Differential Scanning Calorimetry
Queens University Belfast 16/02/12
2
What is a DSC?
Differential: measurement of the difference in heat flow from sample and reference side
Scanning: the common operation mode is to run temperature or time scans
Calorimeter: instrument to measure heat or heat flow.
Heat flow: a transmitted power measured in mW
What is DSC?
3
Ice
Ts Tr
Hot Plate
Heat the hot plate from -20 °C to 30 °C,
What will happen to the ice?
How do Ts and Tr react?
How do the Ts and Tr relate to each other?
Air
DSC working principle
4
Timeor Tr
TemperatureTr
Ts
Tf
Time∆T =Ts-Tr
0
-0.5
Tf
DSC raw signal
DSC working principle
5
DSC working principle
DSC raw signal,
Timeor Tr
∆T =Ts-Tr
0
-0.5
Tf
Timeor Tr
Heat flow (mW)
0
-10DSC signal,
Peak integral -> ∆H
=∆T/Rth
Rth, thermal resistence of the system
∆H
6
Baseline slope
Where,
m is the sample masscp is the specific heat capacity of the sample is the heating rate
Timeor Tr
Heat flow (mW)
0
-10
Initial deflection
A normal DSC curve is not horizontal, its baseline shows a slope.
β pcm
7
ICTA and Anti-ICTA
ICTAC (International Confederation for Thermal Analysis and Calorimetry)
Direction of DSC signal
melting
In, 6.0000 mg
mW
-20
-10
0
°C120 130 140 150 160 170
exo
STARe SW 9.10MSG Lab: NJ
melting
In, 6.0000 mg
mW
0
5
10
15
20
°C120 130 140 150 160 170
endo
STARe SW 9.10MSG Lab: NJ
ICTA (∆T=Ts-Tr) endothermic downwards,
exothermic upwards.
Anti-ICTA (∆T=Tr-Ts) endothermic upwards, exothermic downwards.
8
Endothermic and exothermic effects
Endothermic:
When the sample absorbs energy, the enthalpy change is said to be endothermic. Processes such as melting and vaporization are endothermic.
Exothermic:
When the sample releases energy, the process is said to be exothermic. Processes such as crystallization and oxidation are exothermic.
9
Exothermic effect
DSC raw signal
Timeor Tr
TemperatureTr
Ts
Time
0
∆T =Ts-Tr
10
Schematic DSC curve of a polymer
1 23 4 5
6
Tem perature
He
at f
low
e xo
endo
1. initial startup deflection; 2. glass transition; 3. crystallization; 4. melting; 5. vaporization; 6. decomposition.
11
What is melting and crystallization?
amorphouscrystalline
Melting of Indium: 156.6 °C, -28.6 J/g (endothermic)
Crystallization of Indium: 153.5 °C, +28.6 J/g (exothermic)
12
In: 6.18 mg10 K/min
Integral -193.95 mJ normalized -28.52 Jg -1Onset 156.58 °C
Integral 194.27 mJ normalized 28.57 Jg -1Onset 153.43 °C
mW
-10
0
10
20
°C140 145 150 155 160 165
exo prod 1 13.03.2006 13:58:29
STARe SW 9.01MSG2006: Marco
Melting and Crystallization with DSC
13
How to evaluate melting peaks
• Pure materials:
- onset (independent of heating rate)
- Hf baseline: line, integral tangential
• Impure materials:
- peak temperature (depends on )
- Hf baseline: line, tangential right - purity analysis for eutectic systems (based on curve shape analysis)
• Polymers
- peak temperature (depends on and m)
- Hf baseline: line, spline, integral tangential
14
amorphous solid,rigid, brittle
liquid (non polymers)rubber like (polymers)
What is glass transition?
Glass transition is cooperative molecular movement.
Glassy state Rubbery stateGlass transition
15
The glass transition with DSC
dT
dH
mcp
1
pcm
Temperature
cp
Temperature
ex
othe
rm
16
Chemical reaction
A chemical reaction is a process that one or more substances (reactants) are converted to one or more new chemical substances (products) with different properties. e.g. oxidation, decomposition, polymerization etc.
Chemical reactions always involve a change in energy. Depending on whether the energy is absorbed or released during the process, they can be endothermic or exothermic.
17
Chemical reaction
Homogeneous decomposition of dibenzoyl peroxide; peak temperature and peak shape depend on heating rate; peak area is independent of heating rate.
18
Materials
Additives
Plasticizers
Impurities
Fillers
Processing
Thermal treatment Mechanical stressing
Shaping Storage and use
MaterialProperties
Where to use DSC?
Polymers
Pharmaceuticals
Chemicals
Food
Cosmetics
19
DSC
Multiple Thermocouples increase sensitivity and reduce noise
For Best Resolution: Low signal time constant e.g 1.7 s (20-μL Al crucible, N2 gas)
High baseline stability using chemically resistant ceramic substrate and relatively inert silver furnace
Resolution and Sensitivity
20
Sensor technology
TSR
S R Temperature gradients on the sensor lead to baseline deviation from zero
TR0 TS0
S R T0
A single sensor temperature (T0) is measured.
Inhomogeneous temperature distribution of the sensor is not considered.
21
Inner ring of thermocouples measure TR and TS
Outer ring measures sensor temperatures at reference and samples sides, TS0 and TR0
Thermocouples act as thermal resistence, R.
TS
S R
TSTR
TS0 TR0
Sensor technology
22
Heat flow on the sample and reference sides are separately measured
N is the number of thermocouples (TC) per ring.FRS5 sensor (56 TC): N = 14
HSS7 sensor (120 TC): N = 30
TS
S R
TSTR
TS0 TR0
00 RSdt
dq
N
i i
iSiSS R
TT
1
,0,0
N
i i
iRiRR R
TT
1
,0,0
Sensor technology
23
Noise and sensitivity
Peak Height 137 uW
Lysozyme dissolved in 0.1 M HCl/glycinebuffer at pH = 3Heating rate 3 K/minSample Mass around 105 mg
1.7 % Lysozyme
uW100
°C50 60 70 80 90
Peak Height 6.5 uW
Step 0.69 uW
0.1 % Lysozyme
uW5
min
°C60 65 70 75 80
18 20 22 24
exo Lysozyme 1.7% and 0.1% 29.01.2008 16:41:22
STARe SW 9.10MSG Lab: NJ
24
Noise and sensitivity
25
Resolution
26
How long does the system take to equilibrate?
How fast does the signal come back to the baseline?
Small Signal better resolution
Signal = RthCs, Cs = Cpan+ Csample+ Csensor
FRS5 sensor (Rth 0.04 K/mW) & Al40 l (50 mg)
Cpan 50 mJ/K
Csample (10 mg, 1.5 J/gK) 15 mJ/K => Signal 3 s
Csensor 10 mJ/K
FRS5 sensor (Rth 0.04 K/mW) & Al20 l (20 mg)
Cpan 20 mJ/K => Signal 1.8 s
Signal time constant
27
Signal time constant
How to improve Signal?
Cs can be strongly influenced by the choice of the pan.
Recommendations for better resolution:
-> Al20 ul pan instead of Al40 ul pan
-> Al pans instead of alumina pans
Cs can be reduced by using smaller sample size
Signal can be further decreased by using He as purge gas.
28
Cooling behavior