Urea Reactor Explosion Accident Stress Corrosion Analysis
Zhonghe Chen1,a, Weiqiang Wang2,b, Mingda Song2,c ,Ningning Dong1,a
1School of Chemistry and Chemical Engineering, University of Jinan, Jinan 250022, China;
2School of Mech. Eng., Shandong University, Jinan 250061, China
Key words: urea reactor; explosion; fracture analysis; stress corrosion
Abstract: In order to find out the accident urea reactor explosion reasons, based on the accident
investigation, the reactor structure was anatomyed, the macroscopic and microscopic fractures were
sampled and observed, The results show that the trace sodium, potassium and other alkaline ions
content in the liquid of liquefied steam is the stress corrosion medium reason; the leak detection pine
and the 16MnR laminate connecting with screw joint is the structural reasons; typical stress corrosion
had occurred on the accident urea reactor cylindrical segment base metal and welding. Some
important suggestions were given.
Introduction
The urea reactor explosion accident occurred on March 21, 2005 in Shandong Pingyin Chemical
Fertilizer Plant, caused 4 persons to die, 32 persons of severely wounded, the direct economic losses
nearly 30 million Yuan[1]. This accident is extremely similar with the Hebei QianAn Chemical
Fertilizer Plant urea reactor explosion accident 15 years ago. Therefore, we try to carry on the analysis
and research to the accident,tofind out the explosion reasons, operating process, urea reactor structure
and other the correlation questions, will provide the model for the next similar accident prevention.
Urea reactor and accident survey
The accident urea reactor was made in December, 1999, put into the use in March, 2000.The service
examination carried in 2002, the security condition rank decided as 2 levels. This reactor design
pressure is 21.57MPa, the design temperature is 195℃, operating temperature is 188±2℃, actuating
medium is urea solution and ammonium carbamate [1,2]
Multilayer dressing for the reactor structure is made of 10 cylindrical segment and the upper and
lower head components. Multilayer structure is the cylinder, lining layer, blind lamellar, and
11-bandaging laminates. The lining material is the 8mm 316L stainless steel, the blind lamellar
material is 6mm Q235A carbon steel, the inner cylinder material is 12 mm 16MnR low-alloy steel
plate, the bandaging laminates material is 6 to 8 mm 15 MnVR, a total of 11 layers, the total wall
thickness is 110mm (refer with: Fig.1).The reactor length 26.2m, diameter 1400 mm, with a total
weight of 115,210 kg, as class III reaction vessel [1].
The urea reactor suddenly exploded without abnormal signs. The reactor body was exploded into
three sections, the first section is the lower head; the second section is the 9th cylindrical segment,
longitudinal rupture occurred , and torn along the 9th cylindrical segment link welding, infiltrated to
the south side main workshop; the third section is the upper head and the 1st to 8th cylindrical
segments, flew away the explosion area more than 90m (refer with: Fig.1-Fig.2).
Investigations shows that the accident occurred under the urea plant functioning properly and
found no abnormal pressure, temperature, media and other records[1].
Advanced Materials Research Vols. 239-242 (2011) pp 156-160Online available since 2011/May/12 at www.scientific.net© (2011) Trans Tech Publications, Switzerlanddoi:10.4028/www.scientific.net/AMR.239-242.156
All rights reserved. No part of contents of this paper may be reproduced or transmitted in any form or by any means without the written permission of TTP,www.ttp.net. (ID: 128.59.222.12, Columbia University Library, New York, USA-12/11/14,03:02:30)
Fig.5 cracking cases
16MnR laminate link
welding
Fracture analysis
Macroscopic fractures analyses
All the fractures between the 9th and 10th cylindrical segment break along the link welding upper
side, also all occured above the link welding base metal area. The entire cross section is quite even
(refer with: Fig.1), many places have longitudinal cracks. The yawn bigger longitudinal crack passed
through the link welding, about 150mm long, the side has the obvious ballooning. The crack beneath
the same thermocouple takeover had a breakthrough before the bursting. This position Q235-A,
16MnR and the inside several 15MnVR steel plate all are the entire even fracture[3,4,5]
(refer with:
Fig.3). Full-face from outside can see the shear direction shear lips, large shear fracture southwest
direction, the radial (outward) shear cracking form.
The 9th cylindrical segment longitudinal fracture surface passed through the thermocouple
takeover hole, in addition to lining, all laminates fracture near the thermocouple takeover hole and
below were brittle fracture [3,5]., and the total cross-section is about 750mm high, and the main fault
near surface crack also can see a large number of vertical cracks cracking obviously, these vertical
cracks in existence before blasting. The main longitudinal fracture surface for the first half of the
ramps fracture toughness, fracture near every laminate did not see other cracks (refer with: Fig.4).
After bursting, the cylindrical segment along the wall outside the aforementioned profile stack
together, the laminates thickness there was no significant change. Around the leak detection hole, the
neighbor number layers plate have the obvious radiated dehiscence cracks [3] (refer with: Fig.5).
The fracture between the 8th and 9th cylindrical segment near the inside lining almost all to be
located on the link welding upper side , only a small area is situated at the lower side, while section
near the outer side is mainly at the lower side. Internal evener fracture is situated at laminates to the
southwest, nearly 10 layers, and from southwest to northeast gradually reduced, at least there are two
layers. The northeast outer fracture section is located at the weld lower side, in addition to the three
inner lining layers broken on the upper side of the link welds. After observation and survey, the cross
section and the nearby reactor diameter and various layers thickness has had no remarkable change.
The tray of 1st~8th and 10th cylindrical segment support welds on the inside lining mostly has
the distortion, the distortion direction all aims at the fracture to outside. Apart from the top cylindrical
segment tray stay in the in-situ, the others flew outside. Inspection on inner lining surface, we
discovered the welding and the head pile welded layer is the bright white color, the base metal surface
is brown or the ash black, the inner lining surface has no cracks. Except that nearby the 9th cylindrical
segment thermocouple hole partial and 8th, 9th cylindrical segment link welding, few macroscopic
even fractures, the other lining fracture all were the shear fracture. [4,5]
Sampling upward from 8th cylindrical segment bursting fracture, we found that there are obvious
laminates longitudinal crack, we discovered that similar serious longitudinal crack exists on the
laminates base metal, the crack penetrated 4 layers, the crack length up to 450 mm, the actual crack
continues from the sample place to the link welding direction to extend. At the same time, in 7th and
Fig.1 10th cylindrical
segment and its fracture
Fig.2 9th cylindrical
segment morphology
Fig.4 morphology of
tear into 8th cylindrical
segment
Fig.3 the radial cracks
around the leak detection
hole
Advanced Materials Research Vols. 239-242 157
Fig.6 the link welding
cracking case of 7th and
8th the leak detection hole
8th cylindrical segment, the link welding neighboring the sampling leak detection hole, also
discovered the parallel weld crack, cracks expanded from welding line to welding toe, including
Q235-A, 16MnR and 15MnVR four layers of plate[5,6] (refer with: Fig. 6).
Based on the above analysis and macro fracture anatomy test results, we found no obvious macro
manufacturing defects presence in the welding, there were serious longitudinal and the crosswise
cracks before the explosion, in 9th cylindrical segment near the thermocouple hole there were initial
longitudinal cracks long about 900 mm, penetrating all laminates except the inside lining,
longitudinal cracks in the cylindrical segment is the most serious.
Micro-fracture analysis
We carried analysis on the fracture and the crack microscopic fracture to the 8th~10th cylindrical
segment. Fig.7 to 9 is the 8th and 9th cylindrical segment sample fracture morphology. They are
obvious signs of corrosion and along crystal fracture morphology of these sites, only in the vicinity of
the crack or fracture near the obvious torn areas to see cleavage or dimples fracture, X-ray
spectroscopy analysis showed that corrosion products containing S, Si, K, Ca, Al and other elements [3].
The observation analysis on the burst mouth fracture shows that the fracture morphology is a
typical stress corrosion cracking crack. We carried optical microscopy and scanning electron
microscopy analysis on the sites of link welding area between the two neighboring leak detection
holes 7th and 8th cylindrical segment, the link welding of 8th cylindrical segment and the fracture and
crack on the base metal. Fig.10 to12 shows that the same crystal crack and bifurcation phenomenon
appeared on Q235-A, 16MnR, 15MnVR materials and their welding. Apart from the Q235-A material
close to lining material, in the fracture along its weld fusion line containing Cr, Ni elements, other
materials inside the corrosion cracks forefront contains Na, K, Cl, P, S, Si, Ca, Mg, Al and other
elements, analysis with the X-ray spectrum. These fractures and the crack profile all have the crystal
dehiscence and furcation's characteristic, simultaneously in the crack has the corrosion product, is the
stress corrosion crack shape characteristic. Fig.13 is the analysis result of 7th and 8th cylindrical
segment link welding profile between the neighboring leak detection holes, it is the typical
morphology of stress corrosion cracking .
Fig.9 torn area and
crack morphology of
15MnVR
Fig.8 fracture
morphology of 16MnR
welding
Fig.7 fracture
morphology of 9th
thermocouple holes
Fig.10 fracture
morphology of 7th
~8th cylindrical
segment Q235-A
158 Advanced Materials, CEAM 2011
Analysis through the blast mouth fracture and the crack profile or the cross section far away the
burst mouth, had proven the urea reactor has already had the massive stress corrosion crack before the
explosion. The link stress corrosion dehiscence crack concentrates to the link welding on leans, but
the longitudinal stress corrosion dehiscence crack concentrates in the 9th cylindrical segment
thermocouple hole below. The stress corrosion dehiscence has caused the reactor body load bearing
cross-sectional area serious insufficiency or in the dangerous section place stress corrosion crack
approaches or surpass the material allowance size, and could easily have destroyed or exploded.
The stress corrosion dehiscence reason
The low stress brittle fracture which caused by the tensile stress and the corrosive medium joint action
is called the stress corrosion. The stress corrosion only under the following specific conditions could
occur: part withstanding tension stress role; has specific corrosive medium environment which
matches with the material category; the material contains impurities or alloy metal.
The stress corrosion medium condition. According to the structural characteristics of urea
reactor, we mainly carry on the analysis from three aspects: First, the stress corrosion crack and the
laminates crevice corrosion products; Second, vent hole exudation; Third, leak detection steam.
Stress corrosion crack and corrosion products in the laminates crevice. We takes samples this
place after wire cutting carries on the electronic exploration needle analysis. Fig.14 is one of the stress
corrosion cracking crevice electron microprobe analysis. The results shown in Tab.1.
Tab.1 analysis results of corrosion products in laminates crevice and stress corrosion crack slit
Analysis Spot Laminates crevice Crack slit
No. 1 2 Average1 2 3 4 5 Average
Na element content %
6.97 16.11 11.54 0 0.74 1.72 3.99 5.07 2.30
K element content % 4.90 17.95 11.43 1.30 0 0 2.59 0 0.78
Urea reactor body vent hole exudation. Accident investigation found that there was a lot of
exudation in the reactor body vent hole (refer with: Fig.15). We sampled and analyzed the 10th
cylindrical segment vent hole exudation. Analysis shows that, in the exudation Na+ content is 22.1%,
K+ content is 0.12%, Na
+ content is high. Laminates crevice exudation primarily from the
accumulation of leak detection steam, the liquid which discharges from the laminates crevice has the
very high caustic concentration, meets the stress corrosion medium requirement [3]
Leak detection steam
In order to analyze the basic ion ingredient content in the leak detection steam, we carried on the
sample analysis separately on the accident sealed desalting water after the explosion, boiler water, the
steam distribution of the former buffer cans condensed water as well as other 5 urea reactors leak
detection fluid. The analysis results shows that the accident sealed desalting water containing Na+ and
K+, processed by the reverse osmosis water treatment, the final desalting water pH value adjust by
sodium carbonate, therefore Na+ in the steam is understandable.
The leak detection fluid analysis shows that the leak detection solution and the concentration of
ions is very complex, some reactor hazardous ion concentration is still quite high. The factories are
difficult to ensure that the steam cleaner under current technical conditions, which eventually led to
stress corrosion cracking.
Advanced Materials Research Vols. 239-242 159
The ammonia leak testing steam saturation pressure is 1MPa, the temperature is 182°C.
Considering the wall radiation, the water between laminates exists at the liquid state. To each
cylindrical segment the condensation liquid is above link welding upper side; to the entire body, the
condensation water will stress to the lower cylindrical segment.
The above detection and analysis shows that, the stress corrosion cracking cracks and cracks in the
laminates contain higher Na+ , K
+ and other ions, especially in the vent hole exudation Na
+ content is
astonishing high, which meets the stress corrosion medium requirement. At the same time, the final
desalting water pH value adjusted by sodium carbonate, a trace amount of Na+ and K
+ in the steam
enriched in the laminates gap is very shocking[3,6].
The structural conditions caused stress corrosion
Traditional steam leak detection hole structure was designed by hand welding methods to prevent the
leak detection steam leaking to laminates [2].In order to overcome inter-deep hole and laminates
difficult to detect and weld, the screw joint connection way between leak detection pipe and 16MnR
laminates were used, but it is difficult to guarantee seal reliability under the vibration loads and wind
loads, this makes ammonia leakage detection media and the detection steam easily into the
laminates, the appearance of vent hole exudation had proven the detection steam divulges to various
laminates [6].
Conclusion.
Macro-fracture and micro-fracture sampling analysis showed that the explosion reactor existed a lot
of stress corrosion cracks before explosion, and a lot of stress corrosion cracks in base metal zone.
Longitudinal stress corrosion cracking crack beneath the thermocouple hole has exceeded the
capacity limits of size, is a possible explosion fracture origin.
The ingredient analysis on the corrosion product, vent hole exudation, the leak detection fluid and
desalting water indicate that the stress corrosion medium reason is the trace sodium, potassium and
other alkaline ions content in the liquid of liquefied steam. Such enrichment is mutual anastomosis
with the scene of the explosion. The best solution is to abolish the steam leak detection.
The leak detection pine and the 16MnR laminate connecting with screw joint is difficult to
guarantee sealing reliability under the vibration loads and wind loads, which have made a lot of stress
corrosion cracking on laminates, resulting laminate materials serious stress corrosion cracking, this is
the structural reasons of the explosion. The problem of connecting and sealing between leak detection
pine and laminates is still a problem need to study.
References
[1] Iron and Steel Research Institute, Shandong University, et al. Shandong Pingyin Chemical
Fertilizer Plant urea reactor explosion accident investigation report .Jinan,2005. (In Chinese)
[2] L. Vandebroek, F. Verplaetsen, J. Berghmans. Auto-ignition hazard of mixtures of ammonia,
hydrogen, methane and air in a urea plant. Journal of Hazardous Materials, 2002,93(1):123-136
[3] Charlie R. Brooks, Ashok Choudhury. Failure analysis of engineering materials. Beijing:
Machinery Industry Press, 2003. (In Chinese)
[4] Liu Su-e, Zhu ZiYong, Ke Wei. Stress corrosion cracking of a low alloy steel in hot caustic
aluminate solutions.Scripta Metallurgica et Materialia, 1994,31(4):427-432
[5] Novotny Radek, Sevini Filippo, Luigi Debarberis. Testing environmentally assisted cracking of
reactor materials using pneumatic servo-controlled fracture mechanics device. International Journal
of Pressure Vessels and Piping, 2006,83(10):701-706.
[6] H.P. Seifert, S. Ritter. Stress corrosion cracking of low-alloy reactor pressure vessel steels under
boiling water reactor conditions.Journal of Nuclear Materials, 2008, 372(1):114-131.
ou, H.S. Li and X.H. Fang: Cement. Vol. 7 (2002), p. 1-4, In Chinese.
160 Advanced Materials, CEAM 2011
Advanced Materials, CEAM 2011 10.4028/www.scientific.net/AMR.239-242 Urea Reactor Explosion Accident Stress Corrosion Analysis 10.4028/www.scientific.net/AMR.239-242.156
DOI References
[2] L. Vandebroek, F. Verplaetsen, J. Berghmans. Auto-ignition hazard of mixtures of ammonia, hydrogen,
methane and air in a urea plant. Journal of Hazardous Materials, 2002, 93(1): 123-136.
http://dx.doi.org/10.1016/S0304-3894(02)00043-2 [4] Liu Su-e, Zhu ZiYong, Ke Wei. Stress corrosion cracking of a low alloy steel in hot caustic aluminate
solutions. Scripta Metallurgica et Materialia, 1994, 31(4): 427-432.
http://dx.doi.org/10.1016/0956-716X(94)90013-2 [5] Novotny Radek, Sevini Filippo, Luigi Debarberis. Testing environmentally assisted cracking of reactor
materials using pneumatic servo-controlled fracture mechanics device. International Journal of Pressure
Vessels and Piping, 2006, 83(10): 701-706.
http://dx.doi.org/10.1016/j.ijpvp.2006.08.001