    Examples of Steel Fractography

    Professor M Neil James

    [email protected]

    Department of Mechanical & Marine Engineering

    University of Plymouth

    Drake Circus, Plymouth PL4 8AA

    ENGLAND

    mailto:[email protected]:[email protected]
  • 7/29/2019 Fractography Steel

    2/42

    Fractography Resource - [email protected]

    Contents Use the hyperlinks to navigate around this resource

    Fatigue crack growth in moist air

    Fatigue crack growth in vacuum

    Crack growth by hydrogen embrittlement

    Low carbon interstitial-free steels

    Charpy impact fracture

    Fatigue in a high tensile bolt

  • 7/29/2019 Fractography Steel

    3/42

    Fractography Resource - [email protected]

    Fatigue in Air

    Q1N Steel (HY 80)

    0.2C 2.5Ni 1.5Cr 0.5 Mo

    Quenched & Tempered - YS = 653 MPa Grain size 10m vestigial

    striations present

    Linear growth rate

    regime ~ 10-4

    mm/cycle

    Original

    magnification 2kx

  • 7/29/2019 Fractography Steel

    4/42

    Fractography Resource - [email protected]

    Fatigue in Air

    Q1N Steel (HY 80)

    0.2C 2.5Ni 1.5Cr 0.5 Mo

    Quenched & Tempered - YS = 653 MPa Grain size 10m vestigial

    striations present

    Linear growth rate

    regime ~ 10-4

    mm/cycle

    Original

    magnification 5kx

  • 7/29/2019 Fractography Steel

    5/42

    Fractography Resource - [email protected]

    Fatigue in Air

    Q1N Steel (HY 80)

    0.2C 2.5Ni 1.5Cr 0.5 Mo

    Quenched & Tempered - YS = 653 MPa Grain size 10m ductile

    transgranular with some evidence of underlying structure

    Threshold growth

    rate regime ~ 10-7

    mm/cycle

    Original

    magnification 2kx

  • 7/29/2019 Fractography Steel

    6/42

    Fractography Resource - [email protected]

    Fatigue in Air

    Q1N Steel (HY 80)

    0.2C 2.5Ni 1.5Cr 0.5 Mo

    Quenched & Tempered - YS = 653 MPa Grain size 10m ductile

    transgranular with some evidence of underlying structure

    Threshold growth

    rate regime ~ 10-7

    mm/cycle

    Original

    magnification 5kx

  • 7/29/2019 Fractography Steel

    7/42

    Fractography Resource - [email protected]

    Fatigue in Air

    Q1N Steel (HY 80)

    0.2C 2.5Ni 1.5Cr 0.5 Mo

    Quenched & Tempered - YS = 653 MPa Grain size 10m ductile

    transgranular

    Threshold growth

    rate regime ~ 10-7

    mm/cycle

    Original

    magnification 2kx

  • 7/29/2019 Fractography Steel

    8/42

    Fractography Resource - [email protected]

    Fatigue in Air

    Q1N Steel (HY 80)

    0.2C 2.5Ni 1.5Cr 0.5 Mo

    Quenched & Tempered - YS = 653 MPa Grain size 10m ductile

    transgranular with some environment (moisture) induced IG facets

    'Knee' of growth rate

    regime ~ 10-6

    mm/cycle

    Original

    magnification 2kx

  • 7/29/2019 Fractography Steel

    9/42

    Fractography Resource - [email protected]

    Fatigue in Air

    Q1N Steel (HY 80)

    0.2C 2.5Ni 1.5Cr 0.5 Mo

    Quenched & Tempered - YS = 653 MPa Grain size 10m ductile

    transgranular with some moisture-induced oxide build-up by fretting

    'Knee' of growth rate

    regime ~ 10-6

    mm/cycle

    Original

    magnification 1.15kx

    Mechanism of oxide-

    induced fatigue

    crack closure

  • 7/29/2019 Fractography Steel

    10/42

    Fractography Resource - [email protected]

    Fatigue in Air

    Q1N Steel (HY 80)

    0.2C 2.5Ni 1.5Cr 0.5 Mo

    Quenched & Tempered - YS = 653 MPa Grain size 10m ductile

    transgranular with some moisture-induced oxide build-up by fretting

    'Knee' of growth rate

    regime ~ 10-6

    mm/cycle

    Original

    magnification 7.6kx

    Mechanism of oxide-

    induced fatigue

    crack closure

  • 7/29/2019 Fractography Steel

    11/42

    Fractography Resource - [email protected]

    Fatigue in Air

    Q1N Steel (HY 80)

    0.2C 2.5Ni 1.5Cr 0.5 Mo

    Q&T CGHAZ simulation Grain size 58m microstructure has bigger

    influence (e.g. bainite packets) clear IG facets

    Threshold growth

    rate regime < 10-6

    mm/cycle

    Original

    magnification 500x

  • 7/29/2019 Fractography Steel

    12/42

    Fractography Resource - [email protected]

    Fatigue in Air

    Q1N Steel (HY 80)

    0.2C 2.5Ni 1.5Cr 0.5 Mo

    Q&T CGHAZ simulation Grain size 58m microstructure has bigger

    influence (e.g. bainite packets) clear IG facets

    Threshold growth

    rate regime < 10-6

    mm/cycle

    Original

    magnification 500x

  • 7/29/2019 Fractography Steel

    13/42

    Fractography Resource - [email protected]

    Fatigue in Air

    Q1N Steel (HY 80)

    0.2C 2.5Ni 1.5Cr 0.5 Mo

    Q&T CGHAZ simulation Grain size 58m microstructure has bigger

    influence (e.g. bainite packets) ductile transgranular

    Threshold growth

    rate regime < 10-6

    mm/cycle

    Original

    magnification 2kx

    Back to Contents

  • 7/29/2019 Fractography Steel

    14/42

    Fractography Resource - [email protected]

    Fatigue in Vacuum

    Q1N Steel (HY 80)

    0.2C 2.5Ni 1.5Cr 0.5 Mo

    Q&T CGHAZ simulation Grain size 58m no 'knee' in da/dN curve,

    implying no mechanism change over range of growth rate 10-4 to 10-7

    mm/cycle. No IG facets in absence of moist air

    Growth rate ~ 10-4

    mm/cycle

    Original

    magnification 500x

  • 7/29/2019 Fractography Steel

    15/42

    Fractography Resource - [email protected]

    Fatigue in Vacuum

    Q1N Steel (HY 80)

    0.2C 2.5Ni 1.5Cr 0.5 Mo

    Q&T CGHAZ simulation Grain size 58m no 'knee' in da/dN curve,

    implying no mechanism change over range of growth rate 10-4 to 10-7

    mm/cycle. No IG facets in absence of moist air

    Growth rate ~ 10-4

    mm/cycle

    Original

    magnification 2kx

  • 7/29/2019 Fractography Steel

    16/42

    Fractography Resource - [email protected]

    Fatigue in Vacuum

    Q1N Steel (HY 80)

    0.2C 2.5Ni 1.5Cr 0.5 Mo

    Q&T CGHAZ simulation Grain size 58m no 'knee' in da/dN curve,

    implying no mechanism change over range of growth rate 10-4 to 10-7

    mm/cycle. No IG facets in absence of moist air

    Growth rate ~ 10-7

    mm/cycle

    Original

    magnification 500x

  • 7/29/2019 Fractography Steel

    17/42

    Fractography Resource - [email protected]

    Fatigue in Vacuum

    Q1N Steel (HY 80)

    0.2C 2.5Ni 1.5Cr 0.5 Mo

    Q&T CGHAZ simulation Grain size 58m no 'knee' in da/dN curve,

    implying no mechanism change over range of growth rate 10-4 to 10-7

    mm/cycle. No IG facets in absence of moist air

    Growth rate ~ 10-7

    mm/cycle

    Original

    magnification 2kx

  • 7/29/2019 Fractography Steel

    18/42

    Fractography Resource - [email protected]

    Fatigue in Vacuum

    Q1N Steel (HY 80)

    0.2C 2.5Ni 1.5Cr 0.5 Mo

    Q&T - Grain size 10m no 'knee' in da/dN curve, implying no

    mechanism change over range of growth rate 10-4 to 10-7 mm/cycle. No

    IG facets in absence of moist air

    Growth rate ~ 10-7

    mm/cycle

    Original

    magnification 2kx

  • 7/29/2019 Fractography Steel

    19/42

    Fractography Resource - [email protected]

    Fatigue in Vacuum

    Q1N Steel (HY 80)

    0.2C 2.5Ni 1.5Cr 0.5 Mo

    Q&T - Grain size 10m no 'knee' in da/dN curve, implying no

    mechanism change over range of growth rate 10-4 to 10-7 mm/cycle. No

    IG facets in absence of moist air

    Growth rate ~ 10-7

    mm/cycle

    Original

    magnification 5kx

    Back to Contents

  • 7/29/2019 Fractography Steel

    20/42

    Fractography Resource - [email protected]

    Crack Growth by Hydrogen Embrittlement

    Q1N Steel (HY 80)

    0.2C 2.5Ni 1.5Cr 0.5 Mo

    Q&T - Grain size 10m Hydrogen can cause cleavage, quasi-cleavage,

    MVC or IG fracture, depending on crack tip stress, H2 concentration and

    its effect on plasticity

    Quasi-cleavage at

    initiation site

    changes to IG as

    crack tip stress

    decreases

    Bend loading + H2

    charging

    Original

    magnification given

    by micron bar

  • 7/29/2019 Fractography Steel

    21/42

    Fractography Resource - [email protected]

    Crack Growth by Hydrogen Embrittlement

    Q1N Steel (HY 80)

    0.2C 2.5Ni 1.5Cr 0.5 Mo

    Q&T - Grain size 10m Hydrogen can cause cleavage, quasi-cleavage,

    MVC or IG fracture, depending on crack tip stress, H2 concentration and

    its effect on plasticity

    Quasi-cleavage at

    initiation site shown

    at higher

    magnification

    Bend loading + H2

    charging

    Original

    magnification given

    by micron bar

  • 7/29/2019 Fractography Steel

    22/42

    Fractography Resource - [email protected]

    Crack Growth by Hydrogen Embrittlement

    Q1N Steel (HY 80)

    0.2C 2.5Ni 1.5Cr 0.5 Mo

    Q&T - Grain size 10m Hydrogen can cause cleavage, quasi-cleavage,

    MVC or IG fracture, depending on crack tip stress, H2 concentration and

    its effect on plasticity

    Quasi-cleavage at

    initiation site

    changes to IG as

    crack tip stress

    decreases

    Bend loading + H2

    charging

    Original

    magnification given

    by micron bar

  • 7/29/2019 Fractography Steel

    23/42

    Fractography Resource - [email protected]

    Crack Growth by Hydrogen Embrittlement

    Q1N Steel (HY 80)

    0.2C 2.5Ni 1.5Cr 0.5 Mo

    Q&T - Grain size 10m Comparison between IG and cleavage (induced

    by fracture at cryogenic temperatures)

    IG region is on the

    left, and cleavage is

    on the right. Line

    demarcates the

    boundary.

    Original

    magnification givenby micron bar

    Back to Contents

  • 7/29/2019 Fractography Steel

    24/42

    Fractography Resource - [email protected]

    Low Carbon Interstitial-Free Steel

    Typically 0.002C 0.15Mn + Ti, Nb or B additions - YS = 160-200 MPa

    Some of these steels show IG fatigue at low levels of plasticity (e.g. during

    crack initiation, and at long lives)

    Nf

    = 1 196 172

    cycles

    Fatigue performance

    is no worse than

    grades that do not

    show IG fatigue

    Original

    magnification givenby micron bar

  • 7/29/2019 Fractography Steel

    25/42

    Fractography Resource - [email protected]

    Low Carbon Interstitial-Free Steel

    Typically 0.002C 0.15Mn + Ti, Nb or B additions - YS = 160-200 MPa

    Some of these steels show IG fatigue at low levels of plasticity (e.g. during

    crack initiation, and at long lives)

    Nf

    = 1 196 172

    cycles

    Fatigue striations on

    an IG facet

    Original

    magnification given

    by micron bar

  • 7/29/2019 Fractography Steel

    26/42

    Fractography Resource - [email protected]

    Low Carbon Interstitial-Free Steel

    Typically 0.002C 0.15Mn + Ti, Nb or B additions - YS = 160-200 MPa

    Some of these steels show IG fatigue at low levels of plasticity (e.g. during

    crack initiation, and at long lives)

    Nf

    = 1 196 172

    cycles

    Fatigue striations on

    IG facets

    Original

    magnification given

    by micron bar

  • 7/29/2019 Fractography Steel

    27/42

    Fractography Resource - [email protected]

    Low Carbon Interstitial-Free Steel

    Typically 0.002C 0.15Mn + Ti, Nb or B additions - YS = 160-200 MPa

    Some of these steels show IG fatigue at low levels of plasticity (e.g. during

    crack initiation, and at long lives)

    Nf

    = 1 196 172

    cycles

    IG facets at crack

    initiation site

    Original

    magnification given

    by micron bar

  • 7/29/2019 Fractography Steel

    28/42

    Fractography Resource - [email protected]

    Low Carbon Interstitial-Free Steel

    Typically 0.002C 0.15Mn + Ti, Nb or B additions - YS = 160-200 MPa

    Some of these steels show IG fatigue at low levels of plasticity (e.g. during

    crack initiation, and at long lives)

    Nf= 24 371 cycles

    IG facets at crack

    initiation site

    (although damaged

    by surface contact)

    Original

    magnification given

    by micron bar

  • 7/29/2019 Fractography Steel

    29/42

    Fractography Resource - [email protected]

    Low Carbon Interstitial-Free Steel

    Typically 0.002C 0.15Mn + Ti, Nb or B additions - YS = 160-200 MPa

    Some of these steels show IG fatigue at low levels of plasticity (e.g. during

    crack initiation, and at long lives)

    Nf= 24 371 cycles

    Striation growth

    once crack is

    established and

    plasticity levels are

    higher at crack tip

    Original

    magnification givenby micron bar

  • 7/29/2019 Fractography Steel

    30/42

    Fractography Resource - [email protected]

    Low Carbon Interstitial-Free Steel

    Typically 0.002C 0.15Mn + Ti, Nb or B additions - YS = 160-200 MPa

    Some of these steels show IG fatigue at low levels of plasticity (e.g. during

    crack initiation, and at long lives)

    Nf= 24 371 cycles

    Fatigue striations at

    higher magnification

    Original

    magnification given

    by micron bar

  • 7/29/2019 Fractography Steel

    31/42

    Fractography Resource - [email protected]

    Low Carbon Interstitial-Free Steel

    Typically 0.002C 0.15Mn + Ti, Nb or B additions - YS = 160-200 MPa

    An extra-low carbon grade does not show IG fatigue

    Nf= 37 782 cycles

    No IG facets near

    crack initiation site

    Original

    magnification given

    by micron bar

  • 7/29/2019 Fractography Steel

    32/42

    Fractography Resource - [email protected]

    Low Carbon Interstitial-Free Steel

    Typically 0.002C 0.15Mn + Ti, Nb or B additions - YS = 160-200 MPa

    An extra-low carbon grade does not show IG fatigue

    Nf= 37 782 cycles

    Higher magnification

    view of crack

    initiation site

    Original

    magnification given

    by micron bar

    Back to Contents

  • 7/29/2019 Fractography Steel

    33/42

    Fractography Resource - [email protected]

    Charpy Impact Fracture

    Plain medium carbon steel (0.4%C) with a normalised microstructure

    Low temperature

    fracture showing

    cleavage

    Original

    magnification given

    by micron bar

  • 7/29/2019 Fractography Steel

    34/42

    Fractography Resource - [email protected]

    Charpy Impact Fracture

    Plain medium carbon steel (0.4%C) with a normalised microstructure

    Low temperature

    fracture showing

    cleavage twist and

    tilt grain boundaries

    evident

    Original

    magnification given

    by micron bar

  • 7/29/2019 Fractography Steel

    35/42

    Fractography Resource - [email protected]

    Charpy Impact Fracture

    Plain medium carbon steel (0.4%C) with a normalised microstructure

    Ductile fracture at

    room temperature

    showing MVC

    Original

    magnification given

    by micron bar

  • 7/29/2019 Fractography Steel

    36/42

    Fractography Resource - [email protected]

    Charpy Impact Fracture

    Plain medium carbon steel (0.4%C) with a normalised microstructure

    Room temperature

    fracture showing

    MVC and regions of

    brittle inter-pearlitic

    fracture

    Original

    magnification given

    by micron bar

  • 7/29/2019 Fractography Steel

    37/42

    Fractography Resource - [email protected]

    Charpy Impact Fracture

    Plain medium carbon steel (0.4%C) with a normalised microstructure

    Room temperature

    fracture showingMVC at high

    magnification with

    inclusion in hole

    Original

    magnification given

    by micron bar

  • 7/29/2019 Fractography Steel

    38/42

    Fractography Resource - [email protected]

    Charpy Impact Fracture

    Plain medium carbon steel (0.4%C) with a normalised microstructure

    Shear micro-voids

    can occur whereplastic constraint is

    lower, towards the

    specimen edges

    Original

    magnification given

    by micron bar

  • 7/29/2019 Fractography Steel

    39/42

    Fractography Resource - [email protected]

    Charpy Impact Fracture

    Plain medium carbon steel (0.4%C) with a normalised microstructure

    Smooth featureless

    shear can also occurat specimen edges

    Original

    magnification given

    by micron bar

    Back to Contents

  • 7/29/2019 Fractography Steel

    40/42

    Fractography Resource - [email protected]

    Fatigue in a High Tensile Bolt

    High tensile bolt with Q&T microstructure

    Fatigue in bend with

    a slightly reversedcomponent

    Original

    magnification given

    by micron bar

    Back to Contents

  • 7/29/2019 Fractography Steel

    41/42

    Fractography Resource - [email protected]

    Fatigue in a High Tensile Bolt

    High tensile bolt with Q&T microstructure

    Clear striations are

    present in this lowcycle fatigue

    situation; this is the

    reversed bend area.

    Original

    magnification given

    by micron bar

    Back to Contents

  • 7/29/2019 Fractography Steel

    42/42

    Fatigue in a High Tensile Bolt

    High tensile bolt with Q&T microstructure

    High magnification

    view of fatiguestriations in the main

    fatigue region.

    Original

    magnification given

    by micron bar

    Back to Contents