Weld Defect 01

18
3/28/2012 1 Defect of Welding Ir.Soeweify, M.Eng Head of Strength and Structure Groups Department of Shipbuilding Engineering Surabaya Institute of Technology Welding Engineer 1980 Hiroshima University Welding Inspector 1984 Hamburg University Fracture mechanic sertificate 1990 Bandung Institute of Technology Welding defect Metallurgical defect Melting process Incomplete fusion and incomplete penetration Alloying process Slag inclusion and porousity Cristalization process Cold crack and hot crack Dimensional defect Tranversal shrinkage Angular distortion Longitudinal shrinkage Longitudinal distortion

description

thanks

Transcript of Weld Defect 01

  • 3/28/2012

    1

    Defect of Welding

    Ir.Soeweify, M.Eng Head of Strength and Structure Groups

    Department of Shipbuilding Engineering Surabaya Institute of Technology

    Welding Engineer 1980 Hiroshima University Welding Inspector 1984 Hamburg University

    Fracture mechanic sertificate 1990 Bandung Institute of Technology

    Welding defect

    Metallurgical defect Melting process

    Incomplete fusion and incomplete penetration

    Alloying process Slag inclusion and porousity

    Cristalization process Cold crack and hot crack

    Dimensional defect Tranversal shrinkage

    Angular distortion

    Longitudinal shrinkage Longitudinal distortion

  • 3/28/2012

    2

    Weld defect

    Crack

    Incomplete fusion

    Incompl. penetration

    Slag inclusion

    Porosity

    Under cut

    Underfill

    Over lap

    Covexity

    Weld reinforcement

    Arc strike

    Tungten Inclusion

    Spatter

    Delamination

    Lamelar tear

    Seams/lap

    Dimensional

    Defect of Welding

    Metallurgical defect

  • 3/28/2012

    3

    Crack of welding

    Hot crack, Cold crack

    Longitudinal crack, Transversal crack

    Base metal ,Weld metal ,HAZ crack

    Throat, root, toe, under bead, crater crack

    Lamelar tearing

    Hot Crack

    Just start for cristalization

    Segregeration between cristal

    Weld metal crack

    Crack of the first layer

    Creater crack

    Micro crack

    Transversal and logitudinal crack

  • 3/28/2012

    4

    The influence of hot cracking

    Name of

    crack

    Form of crack

    Influence factor for cold

    cracking

    Wcond Chem Rs Bform

    Crack on

    the first

    layer

    V V V V V V V V V

    Dendrite

    crack

    V V V V V V V V V V

    Crater crack V V V V V

    V

    V V

    Hot Crack

    Welding condition

    Chemical composition

    Shrinking load of weld point

    Form of bead

  • 3/28/2012

    5

    Crater crack

    Crater crack occour in the

    end of weld couse of wrong

    welding electrode

    manipulation, Filler metal

    have flow characteristiecs

    with produce concave profile

    when solidification

    Hot crack start from crater

    crack of fillet weld in pipe

    welding, E 308 -16, E 309-

    16, E 316 -16, The welder

    must take care the end of

    welding to full fill the crater

    Crater crack is one of dangerous hot crack

    Preventive Methode of the Hot cracking for each material

    Sensitivity Preventive Methods

    Crack of Weld Metal

    For Material

    For Prose dur

    For De sign

    Kind of Material First Layer

    Crack Dendrit Crack

    Micro Crack HAZ

    Other Crack

    Crack

    In the

    HAZ

    40 Kg/mm2

    Midle sensitive necc to care

    Midle sensitive necc to care

    Low sensitive No Problem

    Midle sensitive necc to care

    Low sensitive No Problem

    50 Kg/mm2

    Midle sensitive necc care

    Midle sensitive necc Care

    Low sensitive No Problem

    Midle sensitive necc care

    Low sensitive No Problem

    60 Kg/mm2

    Midle sensitive necc care

    Midle sensitive necc Care

    Low sensitive No Problem

    Midle sensitive necc care

    Low sensitive No Problem

    70 Kg/mm2

    Midle sensitive necc to care

    Midle sensitive necc to care

    Low sensitive No Problem

    Midle sensitive necc to care

    Midle sensitive necc to care

    C A R B O N S T E E L

    80 Kg/mm2

    Midle sensitive necc care

    Midle sensitive necc care

    Low sensitive No Problem

    Midle sensitive necc care

    Midle sensitive necc to care

    Reduce of P.S Increase of Mn examine of the elememt

    Examine weld condition examine format weld bead.

    Low Shrink age Pre vent Stress

  • 3/28/2012

    6

    Cr- Mo

    Midle sensitive necc care

    Midle sensitive necc to care

    Low sensitive No Problem

    Midle sensitive necc to care

    Low sensitive No Problem

    1Cr Mo

    Midle sensitive necc to care

    Midle sensitive necc Care

    Low sensitive No Problem

    Midle sensitive necc care

    Low sensitive No Problem

    1 Cr Mo

    Midle sensitive necc care

    Midle sensitive necc Care

    Low sensitive No Problem

    Midle sensitive necc care

    Low sensitive No Problem

    2 Cr Mo

    Midle sensitive necc care

    Midle sensitive necc to care

    Low sensitive No Problem

    Midle sensitive necc to care

    Low sensitive No Problem

    3 Cr Mo

    Midle sensitive necc to care

    Midle sensitive necc Care

    Low sensitive No Problem

    Midle sensitive necc care

    Low sensitive No Problem

    5 9 Cr Mo

    Midle sensitive necc care

    Midle sensitive necc to care

    Low sensitive No Problem

    Midle sensitive necc to care

    Low sensitive No Problem

    L O W A L L O Y S T E E L

    Mn - Mo Midle sensitive necc care

    Midle sensitive necc care

    Low sensitive No Problem

    Midle sensitive necc care

    Low sensitive No Problem

    Reduc of P.S Increase of Mn Examined of the elememt

    Examine weld codition Examine format weld bead. Clean Keep enough Slag

    Low Shrink age Pre vent SC

    Preventive Methode of the Hot cracking for each material

    Preventive Methode of the Hot cracking for each material

    Austenit Midle sensitive necc to care

    Midle sensitive necc care

    High sensitive Must care

    Midle sensitive necc care

    Midle sensitive necc to care

    Martensit Midle sensitive necc care

    Midle sensitive necc to care

    Midle sensitive necc to care

    Midle sensitive necc to care

    Midle sensitive necc to care

    S T A I N L E E S

    Ferrit Midle sensitive necc care

    Midle sensitive necc care

    Midle sensitive not care

    High Sensitive Must care

    Midle sensitive necc to care

    Reduc of P.S Increase of Mn Examin of the element Reduced Harmful element Pb,B,O Keep delts ferrite

    Examine weld codition Take of crater Examine format weld bead. Clean Keep enough Slag

    Low Shrink age Prevent Stress Concent

    Pure Nikkel

    High sensitive Must care

    Midle sensitive necc care

    High sensitive Must care

    High sensitive Must care

    Midle sensitive necc to care

    Inconnel High sensitive Must care

    High sensitive Must care

    High sensitive Must care

    High sensitive Must care

    High sensitive Must care

    Hactelloy High sensitive Must care

    Midle sensitive necc care

    Midle sensitive necc care

    High sensitive Must care

    Midle sensitive necc to care

    N I

    B A S E

    Monel High sensitive Must care

    High sensitive Must care

    High sensitive Must care

    High sensitive Must care

    Midle sensitive necc to care

    Reduce PS Increase Mn Reduce Harmful elemen, Pb,B,O Add little element Ti,Nb.Al,Ni Examine element comp

    Examine weld codition Examine format weld bead. Clean Keep enough Slag Apply peening

    Low Shrink age Prevent Stress

  • 3/28/2012

    7

    Cold crack

    Process of crack

    Finish cristalization

    Hydrogen diffusible

    Stress at the weld metal

    HAZ and base metal crack

    Root crack

    Toe crack

    Under bead crack

    Caused of crack

    Chemical composition

    Welding heat input

    Hydrogen diffusible

    Restraint of joint

    Residual stress

    Diforation anggle

    The influence of cold cracking

    Name

    of

    crack

    Form of crack Influence factor for cold

    cracking

    Wh Hdiff Pcm R A Rs

    Root

    crack

    V V V V

    V

    V V

    V

    V V

    V

    V V

    V

    V V V V

    V

    V V V V V

    V

  • 3/28/2012

    8

    The influence of cold cracking

    Name

    of

    crack

    Form of crack

    Influence factor for cold

    cracking

    Wh Hd Pcm R A Rs

    Toe

    crack

    V V V V

    V

    V V

    V

    V V V

    V

    V V V V

    V

    V V V

    The influence of cold cracking

    Name

    of

    crack

    Form of crack

    Influence factor for cold

    cracking

    Wh Hd Pcm R A Rs

    Under

    bead

    crack

    V V V V

    V

    V V V V V V

    V

    Lame

    lar

    tear

    ing

    V V V V V V

    V

    V V

    V

  • 3/28/2012

    9

    Longitudinal and transversal crack

    Longitudinal

    crack start from

    the weld toe in

    the HAZ

    Transvers crack

    start from the

    stop and run of

    weld

    Longitudinal and transversal crack

  • 3/28/2012

    10

    Under bead crack

    Under bead crack

    Some kind of cold

    crack

    Start from the toe of

    weld in HAZ

    Mainly caused by

    Hydrogen diffusible

    Effect of pre heating on root craking

    Experimental results

  • 3/28/2012

    11

    Couse and Prevention Cracks on the HAZ

    Couse

    Base metal have high hardenability

    High C ek and P cm

    C, Mn,Cr conten to high

    Hidrogen diffusible

    Hidrogen Embrittlemen

    High restrain joint

    Preventive

    Chose the lower Cek and Pcm

    Elec. Low hydrogen

    Dry Filler metal

    Clean edge preparation

    Moderate high restrain

    Good weather

    Pre heating and post heating

    Lamelar tearing

    Thick material only

    Delamination first

    High Stress through the

    thickness

    Fillet weld only

    Degree of constraint

    High inclusion of base

    metal

    Low transverse ductility

    High residual stress

  • 3/28/2012

    12

    Lamellar tearing

    Lamellar tearing

  • 3/28/2012

    13

    Lamellar tearing

    Lamelar tearing

  • 3/28/2012

    14

    Lamelar tearing

    Lamelar tearing Lamellar tearing

    Incomplete fusion

    Low heat input

    Travel speed to high

    Amperage to low

    Wrong electrode position

    Weld metal to weld metal

    Weld metal to base metal

  • 3/28/2012

    15

    Incomplete fusion

    Typical side wall incomplete

    fusion

    Incomplete penetration

    Couse of Incomlete penetration Diameter electrode to big Groove angle to small Amperage to low Wrong electrode not deep penetration

    Weld metal does not extend entirely

  • 3/28/2012

    16

    Incomplete penetration

    Incomplete penetration

    on radiography Incomplete penetration

    in root of weld

    Slag inclusion

    Incorrect welding parameter

    Difficult to clean slack

    Molten slack to thick

    Oxidation and deoxidation process

    Unadequate weld preparation

    Iregular visual in X Ray

    Black vision on DT

  • 3/28/2012

    17

    Porosity

    Gas entrapment during solidification

    The least dangerous

    H2S, CO, NO2 Uniformly scattered

    Clustered porosity

    Piping porosity

    Linear porosit

    Dirty base metal

    Under cut

    Under Cut

    Amperage to high

    The wrong welding technique

    Angle of electrode during welding

    Initial crack start from this defect

    Maximum 0.5 mm

  • 3/28/2012

    18

    Under fill

    Over lap

    Over lap

    Protrusion of weld metal beyond the

    weld toe

    Wrong electrode position

    Burn torch