Stress Corrosion Cracking of Duplex Stainless Steels under...
Transcript of Stress Corrosion Cracking of Duplex Stainless Steels under...
1
Stress Corrosion Cracking of Duplex Stainless Steels
under Evaporative Conditions
Mikael SCHÖNNING1, Lena WEGRELIUS
2, Elisabeth JOHANSSON
3,
Rachel PETTERSSON4
1Avesta R&D Center, Avesta, Sweden, [email protected] 2Avesta R&D Center, Avesta, Sweden, [email protected]
3Avesta R&D Center, Avesta, Sweden, [email protected]
4Jernkontoret, Stockholm, Sweden, [email protected]
Abstract
Duplex stainless steels with their ferritic-austenitic microstructure combine many of the beneficial
properties of ferritic and austenitic stainless steels. The duplex microstructure contributes to the high
mechanical strength and high resistance to stress corrosion cracking (SCC). Numerous studies have
shown that duplex stainless steels have excellent resistance to SCC in chloride solutions. However,
little data is available for duplex stainless steel when it comes to chloride induced SCC under
evaporative conditions.
In current study, the chloride induced SCC resistance of different duplex stainless steels grades was
investigated. The studied evaporative SCC test methods include drop evaporation testing, salt spray
slow strain rate testing, as well as long exposure atmospheric field testing. The test results produced by
the authors, as well as relevant literature data are presented, evaluated and discussed with respect to
the suitability of the test methods to rank the SCC resistance of duplex stainless steels under
evaporative conditions.
Keywords
Stainless Steel; Duplex, Stress Corrosion Cracking; Chlorides; Evaporation;
2
Introduction
Aqueous solutions with low concentrations of chlorides normally do not present any problems
to the use of stainless steels. However, localised evaporation of dilute chloride solution can
increase the chloride concentration and lead to pitting corrosion, or even stress corrosion
cracking (SCC) under unfavourable conditions. Splash zones in marine environments, water
lines, wet insulation or dripping water on hot surfaces are examples of conditions where
chloride concentration could build up over time and cause corrosion.
Due to a beneficial combination of the properties from both ferritic and austenitic stainless
steels, duplex stainless steels show high mechanical strength and good resistance to localised
and uniform corrosion [1-5], as well as excellent resistance to chloride induced SCC [6-8].
However, much less data is available for duplex stainless steel when it comes to chloride
induced SCC under evaporative conditions. The aim of current study has been to look into
this subject and to discuss the suitability of various evaporative tests for ranking of the duplex
grades.
Materials
Typical chemical composition, mechanical strength and pitting resistance equivalent (PRE) of
the materials in this work are presented in Table 1 below.
Table 1 Typical compositions and properties of the investigated materials. The mechanical
strength values refer to typical values for hot rolled plate material produced by Outokumpu.
Materials
EN
Designation
Typical chemical composition [wt%] PRE* Rp0.2
[MPa] Rm
[MPa] C N Cr Ni Mo Others
Core 304L/4307 1.4307 0.02 18.1 8.1 18 260 580
Supra 316L/4404 1.4404 0.02 17.2 10.1 2.1 24 260 570
Forta LDX 2101 1.4162 0.03 0.22 21.5 1.5 0.3 5Mn Cu 26 500 700
Forta DX 2304 1.4362 0.02 0.10 23 4.8 0.3 Cu 26 450 670
Forta LDX 2404 1.4662 0.02 0.27 24 3.6 1.6 3Mn Cu 34 520 750
Forta DX 2205 1.4462 0.02 0.17 22 5.7 3.1 35 510 750
Forta SDX 2507 1.4410 0.02 0.27 25 7 4 43 580 830
* PRE = %Cr + 3.3x %Mo + 16x %N
Experimental
Test methods for evaporative conditions that are covered in this study are briefly summarised
in this section.
Atmospheric field testing
The marine exposure sites for the field testing were located in Antwerp in Belgium, Tianjin in
China, Lavéra in France and Dubai in United Arab Emirates. Prior to field exposure the ring
welded specimen coupons (130×130 mm) were pickled. Racks with test specimens were
exposed to a worst case, non-washing marine conditions. Weight loss, type of corrosion and
maximum depth of corrosion attack were evaluated after the field exposure. Further details
can be found in [9, 10].
Wick testing
The Wick test was developed to simulate evaporative conditions by embedding a heated
stainless steel in an insulation material wetted with a dilute chloride solution. The Wick test
method is stipulated in ASTM C692 [11]. The test comprises a U-bend specimen (dry ground
120 grit) that is fitted into a groove of glass fibre insulation material, which is placed in a
3
dilute NaCl solution (1500 pmm chlorides). The level of the solution is controlled and held
stable. The specimen is electrically heated to 100°C. The test duration is 672 hours. After
exposure the specimens are evaluated by visual inspection with optical light microscopy.
Chloride deposit testing in a climate chamber
This test method involves deposition of chloride (0.16 mg/mm2) by
droplets of chloride solution on selected areas of ring welded
specimen. Sixteen droplets were deposited at different areas of the
ring welded samples. These areas were denoted as centre, 1st ring,
2nd
ring, corners, see Figure 1. Samples were exposed in a climate
chamber with different combinations of salt deposit (NaCl, MgCl2,
CaCl2), temperature (30°C, 50°C, 70°C) and relative humidity
(30%. 50%, 70%) for a total of 8 week exposure time. A more
exhaustive test description can be found in [9].
Constant load testing with cyclic salt spray
In order to assess the SCC resistance of welded material, the constant load specimens were
machined from gas tungsten arc welded (GTAW) plates. The flat specimens were of “dog
bone” type. The applied load was 90% of Rp0.2. A cyclic salt spray procedure from the
automotive industry was adopted (ECC1 test by Renault). This salt spray procedure consists
of a number of wet/dry and spray phases. The test was conducted at 50°C & 70°C and the
total test duration was 42 days. The time to failure is recorded. The testing procedure is
further detailed in [9].
Drop evaporation testing (DET)
The drop evaporation test procedure is briefly described below, detailed guidelines are
stipulated in MTI Manual No.3 [12] and ISO 15324 [13]. DET specimen dimensions are
detailed in Figure 2 and a schematic illustration of the test setup in Figure 3. In order to
remove any residual deformation and residual stresses from the machining step, the specimens
were electropolished.
Figure 2 The drawing of a DET specimen, the dimensions
are given in mm.
Figure 3 A schematic
illustration of the DET setup.
The specimen is mounted horizontally between two fixtures. The designated uniaxial load is
applied to the specimen by weights via a steel wire connected to one of the fixtures. The load
is commonly selected to correspond to a stress ratio of 10 to 100% of the Rp0.2 at 200°C. The
specimen is electrically heated to an initial temperature of ≈300°C and an aerated 0.1 M NaCl
solution is dripped onto the middle section of the specimen. The drop frequency is 6 drops per
minute (~0.1 Hz). During a DET cycle the temperature of the specimen fluctuates from
approximately 70°C to 120°C. Unless a failure occurs, the test is terminated after 500 hours.
Time to failure is recorded by a timer connected to the load train.
Figure 1 Overview of
areas where chloride
droplets were deposited.
Center
Corners
Corners
Centre
4
Slow strain rate testing (SSRT) with cyclic salt spray
The cyclic salt spray tests used cylindrical slow strain rate (SSRT) specimens with a diameter
of 3 mm and a 600 grit wet ground surface finish. The strain rate was 2·10-7
s-1
. The specimen
was electrically heated to a maximum temperature of ≈150°C. Every 20th
second 1% NaCl
solution was sprayed, causing the temperature to drop and then gradually increased as the
solution evaporated. This test method is described in more detail in [14, 15]. An advantage of
the cyclic salt spray over the dripping procedure in DET is that contact between the specimen
and the solution is more even and well defined.
Results and Discussion
Apart from high mechanical strength, a recognised key property of duplex stainless steels is
the high resistance to chloride induced SCC. It might seem to be relatively straightforward to
find a test method to discriminate between susceptible materials (e.g. standard 304 & 316-
type austenitic steels) and materials with superior SCC resistance. However, due to the
intrinsic high SCC resistance, ranking of the duplex grades with respect to SCC resistance can
be challenging. This is even more so for test methods designed to represent evaporative
conditions. For instance, a four year atmospheric field testing at several marine sites has had
little success to provoke SCC. None of the tested grades in the reported study, including
duplex grades LDX 2101, DX 2304, LDX 2404 and DX 2205, showed any SCC after 1 and 4
years of exposure [9, 10]. In fact, the marine exposure conditions did not even yield SCC for
the 304L and 316L materials.
Another example is the Wick test results presented in Table 2. The Wick test results clearly
indicate that the duplex grades are resistant, while the standard austenitic grades fail due to
SCC [8]. Thus, it seems that the evaporative conditions in the Wick and atmospheric field
tests are not aggressive enough to rank the duplex grades. Still it should be noted that for
DX 2205 one anomalous case of stress crack initiation was observed. The crack was
reportedly trans-granular and assisted by selective dissolution of the ferrite [16]. None of the
other five specimens showed any sign of cracking.
Table 2 Summary of the test results for the Wick test.
Material Number of specimens
Tested Failed due to SCC
304L 5 5
316L 4 4
LDX 2101 6 0
DX 2304 6 0
LDX 2404 7 0
DX 2205 6 1
Results of climate chamber tests are summarised in Table 3 [9]. Numerous tests at various
temperatures, relative humidity (RH) and different types of salt deposits showed that 304L
and 316L were prone to SCC. The primary mode of corrosion degradation for LDX 2101,
DX 2304 and LDX 2404 was found to be selective dissolution of the ferrite phase. However,
metallographic investigation revealed micro-cracks in all of the tested duplex specimens. The
authors suggested that micro-cracks can accelerate the selective dissolution of the ferrite by
providing an additional transport path for the electrolyte to the underlying ferrite grains. The
proposed designation of such a mechanism was stress-assisted selective corrosion.
Unexpectedly, two of the DX 2205 specimens showed evident stress corrosion cracks when
tested at the most aggressive conditions (70°C, 30% RH, MgCl2 & CaCl2 deposits). The
5
tentative explanation put forward by the authors was that SCC and selective corrosion are two
competing mechanisms and due to higher corrosion resistance of DX 2205 it suffered SCC
when the other duplex grades corroded selectively [9].
Table 3 Average frequency of occurrence for different types of corrosion for ring welded
specimens. A total of 8 weeks exposure in climate chamber with chloride deposits, test data
from [9].
Material
Ring area no.1 Ring area no. 2
% N
o c
orr
osi
on
% E
tch
ing
% P
itti
ng
% S
elec
tive
corr
osi
on
% S
CC
% o
f co
nd
itio
ns
wit
h m
icro
-cra
cks
% N
o c
orr
osi
on
% E
tch
ing
% P
itti
ng
% S
elec
tive
corr
osi
on
% S
CC
% o
f co
nd
itio
ns
wit
h m
icro
-cra
cks
304L 6 6 39 - 48 N/A 10 19 26 - 45 N/A
316L 19 6 39 - 35 N/A 29 10 29 - 32 N/A
LDX 2101 6 31 3 59 0 31 0 53 6 41 0 15
DX 2304 16 29 3 52 0 10 26 29 0 45 0 3
DX 2205 25 28 13 28 6 9 42 19 3 35 0 0
The same work also used the constant load test in combination with cyclic salt spray in a
climate chamber to evaluate the tendency of SCC for duplex LDX 2101, DX 2304 and
DX 2205, as well as 304L and 316L as reference [9]. Welded tensile specimens were used in
this study. With this approach, the authors were able to provoke SCC for 304L test specimens
at both 50°C and 70°C. However, the 316L only exhibited pitting corrosion and the duplex
grades mostly suffered selective ferrite dissolution with some micro-crack initiation at the
HAZ in some cases.
Another candidate test method to rank duplex grades with respect to SCC resistance is the
drop evaporation test (DET). For DET the minimum stress to failure is defined as the lowest
stress level at which a material fails due to SCC. Figure 4 and Figure 5 show the stress to
failure expressed relative to the yield stress (% of Rp0.2 at 200°C) and in absolute terms
(MPa), respectively, for selected duplex grades. As expected, the austenitic grades 304 and
316 were very sensitive to SCC, showing a very low stress to failure (<10% of Rp0.2). Due to
the much higher mechanical strength of the duplex, the difference in SCC resistance is most
striking when comparing the absolute stress values in Figure 5. Despite a higher PRE the
minimum stresses to failure for LDX 2404 and DX 2205 were significantly lower (20 to 30%
of Rp0.2) compared to the lower alloyed LDX 2101 and DX 2304 (50% of Rp0.2). The highest
alloyed duplex grade, SDX 2507, showed the highest stress to failure.
6
Figure 4 The minimum stress to failure of the tested stainless steels expressed in % Rp0.2 at
200°C. At least one test specimen cracked at this load level.
Figure 5 The minimum stress to failure of the tested stainless steels expressed in MPa,
meaning that at least one test specimen cracked at this load level. The error-bars indicate the
scatter due to the variation of the tensile strength between different parent materials (heats).
The lower alloyed duplex grades LDX 2101 and DX 2304 exhibited more general corrosion
compared to the higher alloyed grades LDX 2404, DX 2205 and SDX 2507. In some cases
rupture of LDX 2101 and DX 2304 specimens was caused by significant reduction in cross
sectional area due to excessive general corrosion, as exemplified by Figure 6. The cross
sectional micrograph in Figure 7 clearly shows that the ferritic phase is selectively attacked on
an LDX 2101 specimen. Similar type of selective corrosion has also been seen for grade DX
2304 [17].
0
10
20
30
40
50
60
70
304 316 LDX 2101 DX 2304 LDX 2404 DX 2205 SDX 2507
% R
p0.2
at
20
0°C
DET - Mininum Stress for Failure
0
50
100
150
200
250
300
304 316 LDX 2101 DX 2304 LDX 2404 DX 2205 SDX 2507
Str
ess
[MP
a]
DET - Mininum Stress for Failure
7
Figure 6 Optical cross sectional micrograph of a failed LDX 2101 DET specimen with
general corrosion causing heavy reduction of the cross sectional area.
Figure 7 Optical micrographs showing selective corrosion of the ferritic phase on an
LDX 2101 DET specimen.
The abundant selective dissolution seen for LDX 2101 and DX 2304
is likely to intervene with
the mechanisms of the SCC, resulting in an inhibiting effect. Due to this inhibiting effect the
minimum stresses to failure for LDX 2101 and DX 2304 are inflated, thus the DET results do
not reflect the actual SCC resistance. On the other hand, the higher alloyed materials LDX
2404, DX 2205 and SDX 2507 have a higher resistance to pitting. The higher corrosion
resistance of these grades limits selective corrosion, making the SCC the dominant corrosion
mechanism. As a consequence, the drop evaporation test seems more suitable for ranking
higher alloyed duplex grades, whereas for lower alloyed duplex grades the results should be
evaluated with caution due to inhibiting effect of the extensive selective corrosion on SCC.
For the austenitic steels 304 and 316 on the other hand, the low minimum stress to failure and
relatively short times to failure lead to conclusion that SCC is the predominant corrosion
mechanism, as opposed to pitting corrosion.
Looking at the times to failure for the materials, it is evident that there is some significant
variation, even at the same stress level. For instance, six out of eight DX 2304 specimens
tested at the minimum stress to failure (50% of Rp0.2) failed within 118-470 test hours, but
two specimens did not crack after 500 hours. There are several potential causes for the scatter,
among these is the statistical nature of the SCC itself, which gives an inherent scatter of the
test results. Also, the relatively small cross sectional area of the specimens make them more
susceptible to material defects such as inclusions, rolled-in oxides etc. In addition, test
conditions might vary slightly each time since some initial adjustments might change during
the course of the test (ambient temperature, salt crust formation, fluctuating drop rate etc.).
In an excellent in-depth review of the drop evaporation test by Hitch [18], it is emphasised
that stress-corrosion of stainless steel under evaporative conditions is a complex process.
1.2
7 m
m
0.8
7 m
m
0.7
0 m
m
8
Hitch also highlights some of the essential aspects that have hitherto received little to no
attention in the DET related literature. The most important is the dynamic load contribution
due to cyclic thermal expansion/contraction, which may play some role in crack initiation.
Other factors are the importance of salt crust formation and its influence in the overall
corrosion mechanism, as well as the impact of salt mixes (e.g. seawater) and its implications
on concentration process, salt crust formation and control of test variables.
Some studies employing slow strain rate testing (SSRT) in combination with cyclic salt spray
has also been carried out [14, 15]. An advantage of the cyclic salt spray over the dripping
procedure in DET is that contact between the specimen and the solution is more even and well
defined. The SCC sensitivity evaluated in 1% NaCl cyclic spray is shown in Figure 8 for DX
2304, DX 2205, SDX 2507 and the austenitic stainless steels 304, 310, and 316L.
Figure 8 SCC sensitivity evaluated as ratio of failure elongation in 1% NaCl to failure
elongation under inert conditions. Results from [15].
From the overall SCC sensitivity values it is apparent that all of the tested materials are
sensitive to SCC under these evaporative conditions. For the duplex grades the SCC
resistance seems to increase with increasing PRE. Although the difference in SCC sensitivity
between DX 2304 and DX 2205 is not large, the SDX 2507 is distinctly more resistant.
However, it is very surprising that there is such small difference between the austenitic grades
(304, 310 and 316) and the expectedly much more SCC resistant duplex grades. This could
perhaps be related to the fact that the dynamic loading in SSRT, in combination with the
aggressive environment, leads to perhaps unrealistically severe test conditions [19]. The
cyclic 1% NaCl salt spray causes the specimen temperature to fluctuate between 90°C and
150°C, as well as causing high chloride build-up due to evaporation [14]. These test
conditions are even more aggressive than in DET, where the temperature is somewhat lower
and fluctuates between 70°C and 120°C [17]. The wet-dry cycle is however much shorter – 6
seconds, compared to 20 seconds for the SSRT with cyclic salt spray. It is also worth noting
from results in Figure 8 that the higher alloying levels of chromium and nickel did not make
the austenitic grade 310 more resistant compared to 304 and 316, in fact quite the contrary.
The cause of this is unclear and needs further elucidation.
0
10
20
30
40
50
60
304 310 316 DX 2304 DX 2205 SDX 2507
[%]
SSRT cyclic salts spray 1% NaCl
9
The effect of austenite level on the SCC sensitivity has been investigated by studying a series
of tie-line alloys (0% to 98% austenite) for duplex grade DX 2205 [15]. These alloys had the
same individual phase compositions as for DX 2205 but different proportions of the two
phases. The SCC sensitivity of the tie-line alloys in 1% NaCl cyclic salt spray SSRT is shown
in Figure 9.
Figure 9 SCC sensitivity evaluated as ratio of failure elongation in 1% NaCl to failure
elongation under inert conditions. Results from [15].
The results in Figure 9 indicate that the most extreme austenite levels (0% and 98%) are the
most sensitive to SCC. The highest resistance is seen at 64% austenite, which is somewhat
above the normal ≈50% level for commercially produced DX 2205 material. This clearly
demonstrates a beneficial effect of duplex microstructure on the SCC resistance, compared to
a single phase structure. Nonetheless, it is surprising that the single phase DX 2205 tie-line
alloys have low SCC resistance, especially in the case of the ferritic alloy. Comparing to
Figure 8, it seems that the SCC resistance of the austenitic DX 2205 tie-line alloy is
significantly lower than the 304 and 316 austenitic grades, and on a par with 310. A
metallographic investigation indicated normal microstructure for the tie-line alloys [15]. In
addition, other study in boiling magnesium chloride with same austenitic alloy did not yield
such poor results [20]. This indicates that the austenitic single phase alloy is more sensitive
under evaporative conditions.
Considering the different evaporation test methods discussed above it is evident that choosing
one test method to rank stress corrosion susceptibility of the whole range of duplex grades,
from lean duplex to super duplex, is indeed very challenging. All of the investigated
accelerated laboratory tests bear evidence of selective dissolution of the ferrite as being a key
phenomenon complicating the evaluation of SCC resistance of duplex grades under
evaporative conditions. The selective corrosion and chloride induced SCC are two competing
mechanisms and when selective corrosion dominates, it seems to inhibit the SCC. This is
perhaps most evident when looking at the DET results, but also for Wick test and chloride
deposit tests, where a higher alloyed grade like DX 2205 shows SCC, but lower alloyed lean
duplex grades show less tendency to cracking but suffer heavy selective corrosion. Figure 10
shows the apparent correlation between DET minimum stress to failure and PRE, as well as
0
5
10
15
20
25
30
35
40
45
50
0%
Austenite
30%
Austenite
DX 2205 64%
Austenite
82%
Austenite
98%
Austenite
[%]
SSRT cyclic salts spray 1% NaCl
10
the competing trends of selective corrosion and SCC. The cross-over point, where the SCC
becomes the prevailing corrosion mechanism, appears to be around PRE 34 for LDX 2404.
Figure 10 The PRE of the duplex grades correlated to the DET minimum stress to failure,
also showing the competing trends of SCC and selective corrosion.
Worth a final comment is the potential major impact of surface preparation on the SCC. In a
recent metallography study of stress corrosion cracks on DX 2205 and SDX 2507 drop
evaporation test specimens, Wickström et al. [21] pointed out the importance of the surface
condition. They found that stress corrosion micro-cracks clusters were formed only in the
ferrite phase. Dealloying in the nanocrystalline layer (formed by surface grinding) and
subsequent cracking of the dealloyed layer was considered a precursor to crack propagation
[21]. This is not likely to be an issue for DET testing, for which all specimens were
electropolished, but could be a contributory factor in other cases.
Conclusions
From the results presented in the current study and analysed literature data, the following
conclusions can be drawn:
Stress corrosion cracking under evaporative conditions is a complex process, which
makes it very challenging to simulate such conditions in an accelerated laboratory test
Very aggressive test conditions are necessary to induce SCC for duplex stainless steel
in order to obtain a relative performance ranking
The ferritic-austenitic microstructure makes the duplex stainless steels very resistant to
chloride induced SCC, especially compared to 304 and 316-type austenitic grades
Under evaporative conditions selective dissolution of the ferrite and SCC are two
competing mechanisms. Selective corrosion can inhibit SCC for lower alloyed duplex
stainless steels when it is the dominant corrosion mechanism
Due to the crack-suppressing effect of selective corrosion, the drop evaporation test
seems to be most appropriate for duplex grades with PRE ≥ 34. For lower alloyed
duplex grades the results might be inflated and should be regarded with caution.
20
25
30
35
40
45
50
0
10
20
30
40
50
60
70
LDX 2101 2304 LDX 2404 DX 2205 SDX 2507
PR
E
% R
p0.2
at
20
0°C
DET - Miniumum stress level for failure PRE
11
References
1. Outokumpu Corrosion Handbook. 11th ed, ed. O.S. AB. 2015: Outokumpu Oyj.
2. Wallén, B., Corrosion of Duplex Stainless Steels in Seawater. Acom, 1998(1): p.
1-11.
3. EuropeanCommission, Avoiding catastrophic corrosion failure of stainless steels
(CORINOX). 2011, Directorate-General for Research and Innovation.
4. Canderyd, C., A. Bergquist, and R. Pettersson, Uniform Corrosion of Lean Duplex
Stainless Steel Compared to Standard Austenitic Grades, in Eurocorr. 2009: Nice.
5. Mameng, S., Localised corrosion of stainless steels depending on chlorine dosage
in chlorinated water, in Eurocorr. 2011: Stockholm.
6. Pettersson, R. and E. Johansson, Stress corrosion resistance of duplex grades.
Acom, 2011(1): p. 10-22.
7. European Commission, Stress corrosion cracking in newer stainless steel grades.
2002, Directorate-General for Research and Innovation.
8. Johansson, E. and T. Prošek, Stress corrosion cracking properties of UNS 32101 -
a new duplex stainless steel with low nickel content. Acom, 2007(2): p. 2-13.
9. EuropeanCommission, Duplex stainless steel in storage tanks (DUPLEXTANK).
2013, Directorate-General for Research and Innovation.
10. Le Gac, A. and N. Le Bozec, Duplex stainless steel in storage tanks (contract
work). 2015, Institut de la Corrosion: Brest.
11. ASTM, Standard Test Method for Evaluating the Influence of ThermalInsulations
on External Stress Corrosion Cracking Tendency of Austenitic Stainless Steel in
ASTM C692. 2006, ASTM International: West Conshohocken.
12. MTI, Guideline Information on Newer Wrought Iron- and Nickel-base Corrosion
Resistant Alloys—Phase 1, Corrosion Test Methods, in Method MTI-5, Appendix
E, MTI Manual No. 3. 1980, Materials Technology Institute of the Chemical
Process Industries Inc.
13. Corrosion of metals and alloys - Evaluation of stress corrosion cracking by the
drop evaporation test, in BS EN ISO 15324:2008. 2008, European Committee for
Standardization - CEN.
14. Linder, J. and R. Pettersson, Slow strain rate testing of duplex stainless steels
under spray evaporation conditions. 1996, Swedish Institute for Metals Research:
Stockholm.
15. Wessman, S.M. and R.F.A. Jargelius-Pettersson, SSRT testing of stainless steels by
spray evaportation in NaCl environment. 1998, Swedish Institute for Metals
Research: Stockholm.
16. Andersen, H., et al., SCC of Stainless Steel Under Evaporative Conditions. Acom,
1998(3): p. 1-13.
17. Arnvig, P.-E. and W. Wasielewska, Stress Corrosion Behaviour of Highly Alloyed
Stainless Steels under Severe Evaporative Conditions. Acom, 1993(3): p. 1-7.
18. Hitch, D.C.A., Stress-Corrosion Cracking of Duplex Stinaless Steel in
Evaporating Seawater, in Corrosion and Protection Centre. 1997, University of
Manchester Institute of Science and Technology (UMIST): Manchester. p. 124.
19. Kivisäkk, U.H. and G. Chai, Influence of Test Method and Relaxation on the
Result from Stress Corrosion Cracking Tests of Stainless Steels in Dilute Neutral
Chlorides. Corrosion, 2003. 59: p. 828-835.
12
20. Jargelius, R.F.A., et al. Chloride Induced Stress Corrosion Cracking of Duplex
Stainless Steel in Concentrated Chloride Environments. in Proceedings DSS '91.
1991. Beaune France.
21. Wickström, L., et al., Microcrack clustering in stress corrosion cracking of 22Cr
and 25Cr duplex stainless steels. Corrosion Science, 2016. 109 (August 2016): p.
86-93.