Progress of Cast Superalloys at NETL · 2017. 3. 23. · superalloys •Identify and select...
Transcript of Progress of Cast Superalloys at NETL · 2017. 3. 23. · superalloys •Identify and select...
![Page 1: Progress of Cast Superalloys at NETL · 2017. 3. 23. · superalloys •Identify and select materials capable of withstanding creep, fatigue and corrosion at 760oC (1400oF) at 35](https://reader035.fdocuments.us/reader035/viewer/2022071502/61217c64f7c4f9228866e777/html5/thumbnails/1.jpg)
Progress of Cast Superalloys at
NETLP. D. Jablonski, K. A. Rozman,
M. Detrois, J.A. Hawk, J. S. Sears
March 2nd, 2017
![Page 2: Progress of Cast Superalloys at NETL · 2017. 3. 23. · superalloys •Identify and select materials capable of withstanding creep, fatigue and corrosion at 760oC (1400oF) at 35](https://reader035.fdocuments.us/reader035/viewer/2022071502/61217c64f7c4f9228866e777/html5/thumbnails/2.jpg)
2
FUNDING AND SUPPORT
This project is conducted in support of DOE-FE Advanced Combustion, and Advanced Turbine, and Crosscutting Technology Research Programs. The project is executed through NETL Research and Innovation Center’s Advanced Alloy Development Field Work Proposal. This research was supported in part by an appointment of Kyle Rozman to the National
Energy Technology Laboratory Research Participation Program sponsored by the U.S. Department of Energy and administered by the Oak Ridge Institute for Science and Education.
DISCLAIMER
"This report was prepared as an account of work sponsored by an agency of the United States Government. Neither the United States Government nor any agency thereof, nor any of their employees, makes any warranty, express or implied, or assumes any legal liability or responsibility for the accuracy, completeness, or usefulness of any information, apparatus,
product, or process disclosed, or represents that its use would not infringe privately owned rights. Reference herein to any specific commercial product, process, or service by trade name, trademark, manufacturer, or otherwise does not necessarily constitute or imply its endorsement, recommendation, or favoring by the United States Government or any agency thereof.
The views and opinions of authors expressed herein do not necessarily state or reflect those of the United States Government or any agency thereof."
![Page 3: Progress of Cast Superalloys at NETL · 2017. 3. 23. · superalloys •Identify and select materials capable of withstanding creep, fatigue and corrosion at 760oC (1400oF) at 35](https://reader035.fdocuments.us/reader035/viewer/2022071502/61217c64f7c4f9228866e777/html5/thumbnails/3.jpg)
3
• R&D high temperature structural materials for power generation
• Focus on Steels and Ni-superalloys
• Identify and select materials capable of withstanding creep, fatigue and corrosion at 760oC (1400oF) at 35 MPa (5000 PSI)
• Melt facility capable of• 300 lb VIM and Air melting• 20, 30, 50 lb VIM• 3, 4, 6 and 8” VAR/ESR
NETLMaterials focus and some processing capabilities
![Page 4: Progress of Cast Superalloys at NETL · 2017. 3. 23. · superalloys •Identify and select materials capable of withstanding creep, fatigue and corrosion at 760oC (1400oF) at 35](https://reader035.fdocuments.us/reader035/viewer/2022071502/61217c64f7c4f9228866e777/html5/thumbnails/4.jpg)
4
• Steam turbine rotors are typically cast into an ingot form then forged and machined to final dimension
• The window of hot working some superalloys is only 100oC, preventing the forging process
• If we could eliminate the forging process manufacturing costs could be lowered
• Rotors typically aren’t cast to size because of segregation and grain size considerations.
• Billets are forged and extruded for pipe and tubing.
• Other components such as turbine casings and valve chests are cast due to their complex geometry.
ManufacturingSome background on steam plant components
Forging of power transmission shaft,Screenshot of youtube video, copyright is by Saarschmiede GmbH Freiformschmiede in Germany
https://www.youtube.com/watch?v=mnCKGI7Fnm8
Forging
Rotor Shaft
50,000 lb Casting
![Page 5: Progress of Cast Superalloys at NETL · 2017. 3. 23. · superalloys •Identify and select materials capable of withstanding creep, fatigue and corrosion at 760oC (1400oF) at 35](https://reader035.fdocuments.us/reader035/viewer/2022071502/61217c64f7c4f9228866e777/html5/thumbnails/5.jpg)
5
• IN740H is a derivative of Nimonic 263 intended for structural use in high temperature applications/boiler side
• Gamma prime strengthened• Minimal Eta formation
• Boiler certified• UNS # N07740• Approved by Code Case 2702 under
ASME B31.1 by Code Case 190• Max temperature 800oC
Inconel 740HWork on cast H282 has been successful; Update on a cast version of IN 740H
Shingledecker, J.P. et al., Mat. Sci. Engr. A 578 (2013) 277‐286
E lement Mn S i C r Ni C o Mo Nb T i Al F e C u P T i+Al+Nb T i:Al C N O S B L aMin 0 0 23.5 bal 15 0 0.5 0.5 0.2 0 0 0 1.20 2.5 50 ‐ ‐ 0 6 ‐
Nominal 0 0.15 24.5 bal 20 0.1 1.5 1.35 1.35 0 ‐ ‐ 4.20 1 300 ‐ ‐ ‐ ‐ ‐Max 1 1 25.5 bal 22 2 2.5 2.5 2 3 0.5 0.03 7.00 1.25 800 ‐ ‐ 300 60 ‐
PPM% Wt S treng thener
Twin
ASTM #3 grain size γ'
![Page 6: Progress of Cast Superalloys at NETL · 2017. 3. 23. · superalloys •Identify and select materials capable of withstanding creep, fatigue and corrosion at 760oC (1400oF) at 35](https://reader035.fdocuments.us/reader035/viewer/2022071502/61217c64f7c4f9228866e777/html5/thumbnails/6.jpg)
6
• Commercially pure feed stocks used
• Chemistry of pre-alloyed materials tightly controlled• NiCrLa, NiB, Ni-50Cr, Ni-30Co-30Cr
• Vacuum / Ar atmosphere melt and pour
• Cast IN740H into 4” graphite mold with slow cooling
• Computationally based homogenization and aged • 1120oC/ 1hr /AC / 850oC/16hr• Simulates thick wall sections• *Not forged*—cast structure
• Extracted tensile and creep samples from 4” round
• Test mechanical properties• Followed ASTM standards
• Tracked columnar and equiax location of samples
Mechanical TestingResults from the 4” round test
4”
![Page 7: Progress of Cast Superalloys at NETL · 2017. 3. 23. · superalloys •Identify and select materials capable of withstanding creep, fatigue and corrosion at 760oC (1400oF) at 35](https://reader035.fdocuments.us/reader035/viewer/2022071502/61217c64f7c4f9228866e777/html5/thumbnails/7.jpg)
7
• All tensile tests from 800oC
• “First Heat casting” shows good strength but poor ductility
• “L1B” shows good ductility but reduced UTS and yield
• “L2B” and “L2C” show intermediate ductility and improved strength
• Columnar grained samples showed slightly higher ductility than Equiaxed samples
• Plotted values are averaged from both orientations
Hot Tensile ResultsFrom the homogenized 4” casting, as per ASTM E7
![Page 8: Progress of Cast Superalloys at NETL · 2017. 3. 23. · superalloys •Identify and select materials capable of withstanding creep, fatigue and corrosion at 760oC (1400oF) at 35](https://reader035.fdocuments.us/reader035/viewer/2022071502/61217c64f7c4f9228866e777/html5/thumbnails/8.jpg)
8
Creep ResultsFrom the homogenized 4” casting, as per ASTM E139
Fit by Shingledecker et al., ~90 samples (Curve)
Shingledecker, J.P. et al., Mat. Sci. Engr. A 578 (2013) 277‐286
NETL Creep samples underperforming(Data points)
750oC
775oC
800oC
• Cast creep samples significantly underperforming compared to wrought alloy
• All temperatures, stresses and heats
• BLACK – 800oC
• RED – 775oC
• BLUE – 750oC
![Page 9: Progress of Cast Superalloys at NETL · 2017. 3. 23. · superalloys •Identify and select materials capable of withstanding creep, fatigue and corrosion at 760oC (1400oF) at 35](https://reader035.fdocuments.us/reader035/viewer/2022071502/61217c64f7c4f9228866e777/html5/thumbnails/9.jpg)
9
Creep ResultsFrom the homogenized 4” casting, as per ASTM E139
Shingledecker, J.P. et al., Mat. Sci. Engr. A 578 (2013) 277‐286
NETL, rupture ductility
• Cast creep samples have significantly less rupture ductility than wrought samples
• All temperatures, stresses and “heats”
• Ductility <5%
• Unacceptable for structural materials
• BLACK – 800oC
• RED – 775oC
• BLUE – 750oC
![Page 10: Progress of Cast Superalloys at NETL · 2017. 3. 23. · superalloys •Identify and select materials capable of withstanding creep, fatigue and corrosion at 760oC (1400oF) at 35](https://reader035.fdocuments.us/reader035/viewer/2022071502/61217c64f7c4f9228866e777/html5/thumbnails/10.jpg)
10
• Chemistry within spec, although high sulfur (100 PPM)
• Heat A showed poor ductility
• Analysis of the original casting showed angular particles rich in Nb, C and S, likely Carbosulfides
• Could it be that sulfur was causing the low ductility?• Lanthanum was subsequently added to strip the sulfur
from input materials• Results indicate sulfur levels below 10 ppm
AnalysisOriginal casting “A”
Gedds, Leon and Huang, Superalloys Alloying and Performance, 201, ASM international, ISBN 0615030409, p41
carbosulfide
20 μm
![Page 11: Progress of Cast Superalloys at NETL · 2017. 3. 23. · superalloys •Identify and select materials capable of withstanding creep, fatigue and corrosion at 760oC (1400oF) at 35](https://reader035.fdocuments.us/reader035/viewer/2022071502/61217c64f7c4f9228866e777/html5/thumbnails/11.jpg)
11
• L1B showed good ductility
• La added to reduce sulfur content• Reduction in sulfur to <10 PPM
• Mo added to modify the carbides
• ~250-500 nm carbides observed• Carbon measured ~300-400 PPM
• Low density of gamma prime• Slight decrease near TiN and
carbides (GB’s)
• No eta phase detected
• Ti, N and La rich phases in matrix and grain boundaries
MicrostructureAs observed from “L1B” heat
Ti, N rich
La richγ'
Carbide
20 μm 1 μm
![Page 12: Progress of Cast Superalloys at NETL · 2017. 3. 23. · superalloys •Identify and select materials capable of withstanding creep, fatigue and corrosion at 760oC (1400oF) at 35](https://reader035.fdocuments.us/reader035/viewer/2022071502/61217c64f7c4f9228866e777/html5/thumbnails/12.jpg)
12
• Fracture morphology appeared inter-dendritic / intergranular
• Significant secondary cracking, not limited to fracture plane
• Observed both in tensile and creep
• ~50% of sample shows ductile fracture
• Consistent with measured ductility
Failure ModeAs observed from “L1B” heat
Ductile failure
IG failure
IG failure
2 mm 5 mm
![Page 13: Progress of Cast Superalloys at NETL · 2017. 3. 23. · superalloys •Identify and select materials capable of withstanding creep, fatigue and corrosion at 760oC (1400oF) at 35](https://reader035.fdocuments.us/reader035/viewer/2022071502/61217c64f7c4f9228866e777/html5/thumbnails/13.jpg)
13
• Carbide morphology appears thick and continues, although jagged
• Not detecting TiN phases from fracture surface
• Ductile dimples are wide and shallow
• Sometimes bright (La) phase at bottom
• Suggesting no influence
• La rich grain boundary precipitates appear near intergranular fractures
• Evidence of IG failure at La rich PPT
• Cleavage failure suggests La rich PPT held GB together until final fracture
• Conclude La rich phases do not influence fracture process
Failure ModeAs observed from “L1B” heat
Shallow ductile dimples
La rich PPT at grain apex
Shallow dimples
IG failure
Cracked La PPT
Jagged carbide
Cleavage failure
TiN
5 μm
20 μm400 μm
![Page 14: Progress of Cast Superalloys at NETL · 2017. 3. 23. · superalloys •Identify and select materials capable of withstanding creep, fatigue and corrosion at 760oC (1400oF) at 35](https://reader035.fdocuments.us/reader035/viewer/2022071502/61217c64f7c4f9228866e777/html5/thumbnails/14.jpg)
14
• L2B increased Ti and Al to yield more gamma prime
• Large 250-750 nm carbides again observed
• Carbon measured ~300-400 PPM
• Ti-N phases on GB and in matrix
• Lath like structure detected• EDS shows Cr rich
• La rich phases detected but not shown here
• L2B showed lower ductility than L1B
MicrostructureAs observed from “L2B” heat
Ti, N richCarbide
γ’
Lath like structure
1 μm20 μm
![Page 15: Progress of Cast Superalloys at NETL · 2017. 3. 23. · superalloys •Identify and select materials capable of withstanding creep, fatigue and corrosion at 760oC (1400oF) at 35](https://reader035.fdocuments.us/reader035/viewer/2022071502/61217c64f7c4f9228866e777/html5/thumbnails/15.jpg)
15
• Mostly intergranular / inter-dendritic failure
• Very limited ductility• When observed
associated with max shear plane
• Similar features observed in both creep and tensile
Failure modeAs observed from “L2B” heat
Ductile failure
IG failure, oriented with max sheer
3 mm 5 mm
![Page 16: Progress of Cast Superalloys at NETL · 2017. 3. 23. · superalloys •Identify and select materials capable of withstanding creep, fatigue and corrosion at 760oC (1400oF) at 35](https://reader035.fdocuments.us/reader035/viewer/2022071502/61217c64f7c4f9228866e777/html5/thumbnails/16.jpg)
16
• Ductility extremely limited• Sub micron size dimples
• Carbide morphology thick and smooth
• Nearly symmetric cracking of La GB PPT
• Further suggests La PPT are not root of failure
• TiN phases detected in centers of grains, with ductile dimple surrounding PPT
• Hypothesis:• The morphology and
location of carbides lead to IG failure with limited ductility as stress is unable to transverse carbides
Failure modeAs observed from “L2B” heat
Smooth carbide
TiN
<1μm dimples
Symmetric cracking
5 μm
20 μm400 μm
![Page 17: Progress of Cast Superalloys at NETL · 2017. 3. 23. · superalloys •Identify and select materials capable of withstanding creep, fatigue and corrosion at 760oC (1400oF) at 35](https://reader035.fdocuments.us/reader035/viewer/2022071502/61217c64f7c4f9228866e777/html5/thumbnails/17.jpg)
17
• Boron was added to strengthen grain boundaries
• Used master alloys absent of La, N
• Absence of TiN and La PPT from previous “heats”
• “Smooth” carbides coat the grain boundaries
• ~250-500 nm in thickness• Carbon measured ~300-400
PPM
• Note: Sample may be over etched, rather than bi-modal γ
MicrostructureAs observed from “L2C” heat
Carbide γ’
Over etch
20 μm 1 μm
![Page 18: Progress of Cast Superalloys at NETL · 2017. 3. 23. · superalloys •Identify and select materials capable of withstanding creep, fatigue and corrosion at 760oC (1400oF) at 35](https://reader035.fdocuments.us/reader035/viewer/2022071502/61217c64f7c4f9228866e777/html5/thumbnails/18.jpg)
18
• Complete intergranular failure observed
• Both creep and tensile samples
• Significant secondary cracking along grain boundaries
Failure ModeAs observed from “L2C” heat
3 mm3 mm
![Page 19: Progress of Cast Superalloys at NETL · 2017. 3. 23. · superalloys •Identify and select materials capable of withstanding creep, fatigue and corrosion at 760oC (1400oF) at 35](https://reader035.fdocuments.us/reader035/viewer/2022071502/61217c64f7c4f9228866e777/html5/thumbnails/19.jpg)
19
• Lath like structure observed on grain facets
• Likely η phase or M23C6 (Cr)
• No η detected from xrd
• No detection of carbides at IG failure
Failure ModeAs observed from “L2C” heat
Micro‐ductility
Lath like structure
Carbide free IG failure
η free GB
20 μm
20 μm400 μm
![Page 20: Progress of Cast Superalloys at NETL · 2017. 3. 23. · superalloys •Identify and select materials capable of withstanding creep, fatigue and corrosion at 760oC (1400oF) at 35](https://reader035.fdocuments.us/reader035/viewer/2022071502/61217c64f7c4f9228866e777/html5/thumbnails/20.jpg)
20
• Work continues to optimize mechanical properties of cast versions of IN740 to improve:
• Low tensile strength
• Low creep ductility
• Niobium rich carbosulfides were detected and eliminated with lanthanum additions
• Poor mechanical properties were measured
• Increase in molybdenum content to eliminate cellular carbide formation
• Somewhat successful in avoiding cellular carbides, however mechanical performance remained poor
• Increase in boron content to enhance grain boundary ductility
• Marginal change in mechanical properties
• Smooth thick carbides tended to reduce mechanical properties while the jagged morphology tended to increase ductility
SummaryObservations from casting IN740H
![Page 21: Progress of Cast Superalloys at NETL · 2017. 3. 23. · superalloys •Identify and select materials capable of withstanding creep, fatigue and corrosion at 760oC (1400oF) at 35](https://reader035.fdocuments.us/reader035/viewer/2022071502/61217c64f7c4f9228866e777/html5/thumbnails/21.jpg)
21
• Decrease grain size to increase the surface area of grain facets / limited by heat conduction
• Would reduce GB carbide thickness—but is difficult to achieve in large castings
• Modify carbides via heat treatment
• Thick carbides appear to be contributing to poor mechanical properties (ductility).
• However, carbides may continue to grow under creep so they need to be stabilized (lower ductility seen in creep)
• Chemistry changes: Fairly tight chemical ranges—the cast version may need to expand beyond the wrought range
• Reduce carbon to < 100 PPM to reduce GB carbide thickness
• (however, higher C generally is better for castability)
• Increase carbide formers; Mo, Nb, Cr, Ti
• Increase boron to 0.01% wt (slightly above specifications, 100 PPM) , or add zirconium (150 PPM) to increase grain boundary ductility
• Increase Ti content, to favor eta plates; expected to act to span grains
• Experiments continue
Future workPossible ways to improve performance
E lement Mn S i C r Ni C o Mo Nb T i Al F e C u P T i+Al+Nb T i:Al C N O S B L aMin 0 0 23.5 bal 15 0 0.5 0.5 0.2 0 0 0 1.20 2.5 50 ‐ ‐ 0 6 ‐
Nominal 0 0.15 24.5 bal 20 0.1 1.5 1.35 1.35 0 ‐ ‐ 4.20 1 300 ‐ ‐ ‐ ‐ ‐Max 1 1 25.5 bal 22 2 2.5 2.5 2 3 0.5 0.03 7.00 1.25 800 ‐ ‐ 300 60 ‐
PPM% Wt S treng thener
![Page 22: Progress of Cast Superalloys at NETL · 2017. 3. 23. · superalloys •Identify and select materials capable of withstanding creep, fatigue and corrosion at 760oC (1400oF) at 35](https://reader035.fdocuments.us/reader035/viewer/2022071502/61217c64f7c4f9228866e777/html5/thumbnails/22.jpg)
22
Thank youQuestions?
ACKNOWLEDGEMENTSThanks to Chris Powell, Matt Fortner, Keith Collins for help and support towards this project
Kyle Rozman, Ph.DPostdoctoral Researcher
Structural Materials Development TeamNational Energy Technology Laboratory