Construction of the fabric - Warp :- 50/36 Bright Size Beam / Weft :- 150/36 CrepeReed 80-84 / Pick 60- 62
The lot size for processing - 2000 mtrs. - (10 kgs. / 100 mtr.)Dyeing machine/liquor volume U - Jet Dyeing machine / 600 ltr.capacity
The Process sequence of Polyester Royal Crepe fabric from grey to the finished stage
Desizing / Scouring Sodium Hydro Sulphite - 500 gms.Caustic Soda - 500 gms.Levocol TFL - 1500 gms.Levocol NID - 500 gms.Temperature 950C./60 mins.
Weight Reduction Sodium Hydro Sulphite - 500 gms.Caustic Soda - 1000 to 5000 gms.Levocol SCR - 1500 gms.Temperature - 1300C./30 mins.
Hot Wash &n Neutralisation Acetic Acid - 1000 gms.Oxalic Acid - 500 gms.Temperature - 80C.-900C./15 mins.
Optical Whitening Or Dyeing White R - X% OWF(pH-4, MLR-1:5) Coralene Dyes - X %
Levocol DFT - 1-2 gpl.Levocol PB - 1.0 gplLevocol PB - 0.5 gpl.Levocol WS - 1.0 gplTemperature - 1300C./30 mins.Levocol DFT - 0.25 gplTemperature - 1300C./30 mins.
Batching for Printing Pad in Levocol PB - 0.3% - 0.5% andHeat set @ - 1800C / 30 sec.
Printing Recipe Coralene Dyes - X %Levocol PB - 1.0 %Levocol KBI - 0.5 % .Levocol HTS - 0.75 %Soft Water - Y %Printex CT-50 - (8% Stock Paste)
Print - Dry - High Temp. Steaming at 1700C./8 minsCold Wash - R. C. - Cold Rinse - Neutralization - Dry
Finishing at 1750C Silicon Softener (12%-14%) Soln - 2% - 3%Epoxy base/Carboxyl base Softener (43% - 45%) - 0.25%Shrinkage - Approx - 12%-14%Final width - 107-112cm.
This process may be modified to suit customer requirement of fabric body and feel
This information is provided in good faith, to the best of our knowledge and without liabili-ties.
Processing & Finishing of Polyester Royal Crepe Fabric
This page is sponsored by : Colourtex Pvt. Ltd.
Email : [email protected]