Measuring Detector Radiation Damagefasffasf Measuring Detector Radiation Damage Jose Luis Salinas,...
Transcript of Measuring Detector Radiation Damagefasffasf Measuring Detector Radiation Damage Jose Luis Salinas,...
fasffasf
Measuring Detector Radiation DamageJose Luis Salinas, Joliet Junior College – CCI Program
Rick J. Tesarek, FermilabAbstract:
Scintillator counters are used as fast accelerator loss monitors. These devices are capable of seeing losses from single RF buckets that are 20 ns apart. The booster uses these fast lost monitors as a tool to understand the beam. [1]. Radiation damage to the optical components of the detectors compromises their performance. The adhesive that is used to make the detectors is most affected. We wish to study how radiation affects the optical properties of the optical cement.
Measuring Transparency: Transparency is the amount of light passing through the sample (RS) divided by the amount of light passing through an empty holder (RE).
Calculate the ratio of the pulse heights the PMTs are giving off when there is no sample.
Now, placing a sample in the setup will change the pulse heights of one of the PMTs. Calculate the ratio.
Results:
0.60.650.70.750.80.850.90.95
1
-‐100 0 100 200 300 400Transm
ission
angle
BC-‐600 #7BC-‐600 #8BC-‐600 #9BC-‐600 #10BC-‐600 #6
0.60.650.70.750.80.850.90.95
1
-‐100 0 100 200 300 400
Transm
ission
angle
EJ-‐500 #1EJ-‐500 #2EJ-‐500 #3EJ-‐500 #4EJ-‐500 #5
Figure 7: Light transmission as a function of the orientation of the sample. Left graph measures BC-‐600. Right graph measures EJ-‐500. The initial angle was set by a mark on the sample. By rotating the sample, we sent light through different parts of the sample to evaluate any imperfections it may contain.
Dosimetry Measurements:
α damage= 3.0x10-‐17 A/cm Φ = fluence I= leakageV = volume
T= Temp (K)kB= Boltzmann constant
Figure 3: Photograph of two samples of optical cement: BC-‐600 (left) from St.-‐Gobain Crystals [2] and EJ-‐500 (right) [3] from Eljen Technologies. The samples are about .300 inch thick and ¾ inch in diameter.
Damage:
Figure 1 shows an FLM. This detector consists of two scintillator bars and two photomultiplier tubes (PMT) and G-‐10 plating. Figure 2 shows two scintillator assemblies that were exposed to radiation. The darkest part of the assembly on the right is the adhesive that sticks the scintillator to the acrylic plastic. We will measure the transparency of the glue samples as a function of radiation exposure .
Test Setup Calibration:We set the gain for each PMT to operate in the linear region. We evaluate the linearity by changing the amount of light the PMT receives by changing the neutral density filter. We then read the pulse height from an oscilloscope.
Transparency Measurements:The transparency measurement setup is illustrated below. We use a 405 nm laser that sends a 40 picosecond wide pulse.
0
0.2
0.4
0.6
0.8
1
1.2
0
0.05
0.1
0.15
0.2
0.25
0.3
0.35
0.4
0.45
0.5
0 0.5 1
P AE /P
BE
Pulse
Height (v)
Filter transmission
PMT A avg
ratio
f
absorberlaser Light
SplitterSample Holder
PMT A(test)
P = pulse heightPMT A = PAE PMT B = PBERatio = PAE /PBE
PMT B(control)
Filter wheel (calibration)
Silicon PhotodiodeWe use a 1 cm x 1 cm x 300 μm thick silicon photodiode to measure radiation dose. The diode leakage current is proportional to the radiation dose and also depends on temperature [4].
References:[1] Woodworth, Brian. “Booster Beam Profile Measurements via Stripping Foil Losses.” FermilabUndergraduate Poster Session, August 11, 2016.[2] Saint-‐Gobain Crystals, 17900 Great Lakes Parkway, Hiram, OH 44234-‐9661[3] Eljen Technology, 1300 West Broadway, Sweetwater, TX 79556[4] Barberis, E. et al. Nucl. Instrum. and Meth. A326 (1993) 373-‐380. [5] www.arduino.cc
I(�) = I(0) + V · � · ↵
I(T ) ⇠ T 2e�1.23(eV)
2kBT
Summary: We developed a test setup that will allow us to measure the transparency of optical cement. We have the equipment to measure the radiation dose and the equipment to measure temperature. We made samples of two different glues and measured its initial transparency before exposing them to radiation. We can now put them into the booster and later on measure the transparency as a function of radiation.
Figure 8: 1 cm x 1 cm x 300 micron silicon diode.
Figure 1: Fast Lost Monitor (FLM). Consists of two black photomultiplier tubes, three green G-‐10 plates, two acrylic plastic pieces (grey area) and two scintillators (blue plates).
Figure 2: Two scintillator assemblies that underwent low (left) radiation dose and high (right) radiation dose. The darkest part of the picture right is the adhesive.
Figure 4: The laser emits a light pulse that is split in half when it passes through a light splitter. One-‐half of the light goes to PMT B and the other half passes through the sample, through a filter wheel, and then into PMT A.
Figure 5: Oscilloscope traces for the reference PMT (yellow) and the test PMT (blue) for three different neutral density filters.
Figure 6: Pulse height vs. filter transmission for PMT operating in linear region.
Glue Samples:
We use a thermocouple attached to an Arduino microprocessor to record the temperature as a function of time [5].
Figure 9: Leakage current as a function of radiation dose from data collected inside CDF detector. Courtesy of CDF Radiation Monitoring Group.
0
5000
10000
15000
20000
25000
30000
0 10000 20000 30000 40000 50000 60000Dose (Gy)
I Leak
(nA)
5/20/15
x8608
Drawing: Counter Assembly 1/7
Name:R.J. Tesarek Phone:
15
20
25
30
19:24:50
19:55:26
20:26:01
20:56:36
21:27:12
21:57:47
22:28:22
22:58:57
23:29:33
00:00:08
00:30:43
01:01:19
01:31:54
02:02:29
02:33:04
03:03:40
03:34:15
04:04:50
04:35:25
05:06:00
05:36:36
06:07:11
06:37:46
07:08:21
07:38:57
08:09:32
08:40:07
09:10:42
09:41:18
10:11:53
10:42:28
Tempe
rature in
celsius
internal Tempexternal Temp
Time
Figure 10: Data collected overnight from Arduino.
PMT PMT
scintillator
G-‐10
acrylic
acrylic acrylic
scintillator scintillator
adhesive