Sizes Current Current Arc time Energy Dep.rate Weight/ Electrodes/ kg Electrodes/Diam. x length range type 1000 pcs. kg weldmetal kg weldmetal
(mm) (A) (s)* E(kJ) H(kg/h) (kg) B 1/N
Welding positions:Diameter(mm) Current(A)
Remarks
Welding parameters, optimum fill passes
Calculation data
Materials to be welded
- per electrode at max. current -
61
Index MDSGritec-B
B3 Stainless and heat resistant steelType Paginanr.
GRINOX 202 62GRINOX 502 64GRINOX 1 66GRINOX 56 68GRINOX 507 70GRINOX 506 72GRINOX 210 74GRINOX 510 76GRINOX 9 78GRINOX 57 80GRINOX 513 82GRINOX 514 84GRINOX 36 86GRINOX 51 88GRINOX 67 90GRINOX 65 92GRNOX 62 94GRINOX 33 96GRINOX 73 98GRINOX 53 100GRINOX 54 102GRINOX 153 104GRITHERM 48 106GRINOX 29 108GRINOX 592 110GRINOX 26 112GRINOX 25 114GRINOX 126 116GRITHERM 44 118GRITHERM 47 120
![Page 2: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/2.jpg)
Diameter (mm)Length (mm)Unit:Pieces / unit (nominal)Net weight/unit (kg)
Classification
Welding positions Current type
Chemical composition (w%), typical, all weld metal and ferritenumber
Mechanical properties, all weld metal
General description
Packaging, available sizes and identification
Identification Imprint: Tip colour:
Liability: All information in this data sheet is based on the best available knowledge, is subject to changewithout notice and can only be considered as suitable for general guidance.
Fumes: Consult information on Welding Safety Sheet, available upon request
Condition Yield strength Tensile strength Elongation Impact ISO-V(J)(N/mm2) (N/mm2) (%)
As weldedRequired AWS A5.4-92
EN 1600-97Typical values
ISO/ASME
Approvals
62
AWS A 5.4-92 : E 308 L-16EN 1600-97 : E 19 9 L R 12
AC/DC electr. +/-
2.5 3.2 4.0 5.0350 350 350 450
box186 115 69 443.9 4.0 3.7 3.7
MDS GRINOX 202 3
GRINOX 202
C Mn Si Cr Ni FN0.020 0.80 0.80 19.5 9.7 4-10
GRINOX 202/308L-16 red
Rutile basic stainless steel electrode for 304L or equivalent steelsExcellent corrosion resistance in oxidizing environments such as nitric acidHigh resistance to intergranular corrosionSmooth bead appearanceEasy slag releaseStrong electrode coatingWeldable on AC and DC
UDT+
+20°C -20°C -196°C
not required min. 520 min. 35 not requiredmin. 320 min. 510 min. 30 not required
440 580 43 70 60 35
PA/1G PB/2F PC/2G PF/3G up PE/4G PF/5G up14253 6
Temperature rangepressure parts: -196...+350°Coxidation resistance: to 800°C
0.2% Proof strength
![Page 3: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/3.jpg)
Sizes Current Current Arc time Energy Dep.rate Weight/ Electrodes/ kg Electrodes/Diam. x length range type 1000 pcs. kg weldmetal kg weldmetal
(mm) (A) (s)* E(kJ) H(kg/h) (kg) B 1/N
Welding positions:Diameter(mm) Current(A)
Remarks
Welding parameters, optimum fill passes
Calculation data
Materials to be welded
- per electrode at max. current -
63
GRINOX 202
Steel grades EN 10088-1/-2 EN 10213-4 W.Nr. ASTM/ACI UNSA240/A312/A351
Extra low carbon X2 CrNi 19 11 1.4306 (TP)304L S30403C<0,03% CF-3 J92500
X2 CrNiN 18 10 1.4311 (TP)304LN S30453Medium carbon 302,304 S30400C > 0,03% X4 CrNi 18 10 1.4301 (TP)304 S30409
GX5 CrNi 19 10 1.4308 CF 8 J92600Ti-, Nb X6 CrNiTi 18 10 1.4541 (TP)321 S32100stabilized (TP)321H S32109
X6 CrNiNb 18 10 1.4550 (TP)347 S34700(TP)347H S34709
GX5 CrNiNb 19 10 1.4552 CF-8C J92710
2.5 x 350 50 - 803.2 x 350 80 - 1104.0 x 350 100 - 1405.0 x 450 140 - 180
1G 2F 2G 3G 4G 5Gup up
2.5 70 70 70 60 60 603.2 100 100 100 70 70 704.0 140 140 140 805.0 180 180 180
For rootpasses DC- is recommended.
![Page 4: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/4.jpg)
Diameter (mm)Length (mm)Unit:Pieces / unit (nominal)Net weight/unit (kg)
Classification
Welding positions Current type
Chemical composition (w%), typical, all weld metal and ferritenumber
Mechanical properties, all weld metal
General description
Packaging, available sizes and identification
Identification Imprint: Tip colour:
Liability: All information in this data sheet is based on the best available knowledge, is subject to changewithout notice and can only be considered as suitable for general guidance.
Fumes: Consult information on Welding Safety Sheet, available upon request
Condition Yield strength Tensile strength Elongation Impact ISO-V(J)(N/mm2) (N/mm2) (%)
As weldedRequired AWS A5.4-92
EN 1600-97Typical values
ISO/ASME
Approvals
64
A rutile-basic all position stainless steel electrode for 304L or equivalent steelsMirror like bead appearanceSelf releasing slagExcellent side wall wetting, no undercutHighly resistant to porosityWeldable on AC and DC
AWS A5.4 : E308L-16*EN 1600 : E 19 9 LR 12 * deviations see remarks
AC / DC electr. +
DB GL TÜV UDT+ 4550 + +
C Mn Si Cr Ni FN0.025 0.75 0.95 19.0 9.7 4-10
+20°C -20°C
not required min. 520 min. 35 not requiredmin. 320 min. 510 min. 30 not required
440 600 45 75 60
1.6 2.0 2.5 3.2 4.0 4.0 5.0250 300 350 350 350 450 450
Box88 278 173 105 68 68 442.7 3.2 3.6 3.7 3.5 4.7 4.5
MDS GRINOX 502 2
GRINOX 502/308L-16 red
GRINOX 502
142536PA/1G PB/2F PC/2G PF/3G up PE/4G PF/5G up
Temperature rangepressure parts: -196...+350°Coxidation resistance: to 800 °C
0.2% Proof strength
![Page 5: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/5.jpg)
Sizes Current Current Arc time Energy Dep.rate Weight/ Electrodes/ kg Electrodes/Diam. x length range type 1000 pcs. kg weldmetal kg weldmetal
(mm) (A) (s)* E(kJ) H(kg/h) (kg) B 1/N
Welding positions:Diameter(mm) Current(A)
Remarks
Welding parameters, optimum fill passes
Calculation data
Materials to be welded
- per electrode at max. current -
65
2.0 x 300 35 - 55 DC+ 40 51 0.59 11.6 151 1.752.5 x 350 45 - 80 DC+ 51 103 0.88 21.7 81 1.753.2 x 350 80 - 115 DC+ 57 177 1.3 34.3 48 1.644.0 x 450 100 - 155 DC+ 83 373 1.8 68.0 24 1.645.0 x 450 150 - 220 DC+ 85 577 2.7 106.2 16 1.67
* stub end = 35mm
1G 2F 2G 3G 4G 5Gup
2.0 45 45 40 40 402.5 70 70 70 60 60 603.2 100 100 100 70 70 704.0 140 140 1005.0 180 180
Deviation: Chemical composition Si max. 1.2% AWS A5.4-92 max. 0.90%
GRINOX 502
Steel grades EN 10088-1/-2 EN 102 13-4 W.Nr. ASTM/ACI UNSA240/A312/A351
Extra low carbon X2 CrNi 19-11 1.4306 (TP)304L S30403C<0,03% CF-3 J92500
X2 CrNiN 18-10 1.4311 (TP)304LN S30453Medium carbon 302,304 S30400C > 0,03% X4 CrNi 18-10 1.4301 (TP)304
S30409GX5 CrNi 19-10 1.4308 CF 8 J92600
Ti-, Nb X6 CrNiTi 18-10 1.4541 (TP)321 S32100stabilized (TP)321H S32109
X6 CrNiNb 18-10 1.4550 (TP)347 S34700(TP)347H S34709
GX5 CrNiNb 19-10 1.4552 CF-8C J92710
![Page 6: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/6.jpg)
Diameter (mm)Length (mm)Unit:Pieces / unit (nominal)Net weight/unit (kg)
Classification
Welding positions Current type
Chemical composition (w%), typical, all weld metal and ferritenumber
Mechanical properties, all weld metal
General description
Packaging, available sizes and identification
Identification Imprint: Tip colour:
Liability: All information in this data sheet is based on the best available knowledge, is subject to changewithout notice and can only be considered as suitable for general guidance.
Fumes: Consult information on Welding Safety Sheet, available upon request
Condition Yield strength Tensile strength Elongation Impact ISO-V(J)(N/mm2) (N/mm2) (%)
As weldedRequired AWS A5.4-92
EN 1600-97Typical values
ISO/ASME
Approvals
66
AWS A-5.4-92 : E308 L-15EN 1600-97 : E 19 9 L B 22
DC elec. +
DB TÜV UDT+ + +
C Mn Si Cr Ni FN0.025 1.8 0.4 19.0 10.0 4-10
2.5 3.2 4.0350 350 350
Box191 122 823.8 3.8 4.0
MDS GRINOX 1 3
GRINOX 1 / 308L-15 red
GRINOX 1
Temperature rangepressure parts: -196...+350°Coxidation resistance: n.a.
Chemical composition (w%), typical, all weld metal and ferritenumber
+20° -196°C
not required min. 520 min. 35 not requiredmin. 320 min. 510 min. 30 not required
450 600 40 80 40
142583PA/1G PB/2F PC/2G PF/3G up PG/3G down PE/4G
Basic coated electrode for low temperature applicationsLow carbon content, good impact properties down to -196°CGood weldability and smooth bead appearanceHigh resistance against oxidation up to 800°CWelding on DC electrode+ is recommended
DC electr. +
0.2% Proof strength
![Page 7: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/7.jpg)
Sizes Current Current Arc time Energy Dep.rate Weight/ Electrodes/ kg Electrodes/Diam. x length range type 1000 pcs. kg weldmetal kg weldmetal
(mm) (A) (s)* E(kJ) H(kg/h) (kg) B 1/N
Welding positions:Diameter(mm) Current(A)
Remarks
Welding parameters, optimum fill passes
Calculation data
Materials to be welded
- per electrode at max. current -
67
GRINOX 1
2.5 x 350 55 - 65 DC+ 50 86 0.82 19.1 88 1.893.2 x 350 70 - 90 DC+ 51 135 1.3 31.6 53 1.724.0 x 350 90 - 120 DC+ 66 206 1.7 47.0 32 1.565.0 x 450 110 - 140
* stub end = 35mm
1G 2F 2G 3G 4G 5Gup up
2.5 60 60 60 60 60 603.2 95 90 90 75 75 754.0 125 110 125 100 100 100
Steel grades EN 10088-1/-2 EN 10213-4 W.Nr. ASTM/ACI UNSA240/A312/A351
Extra low carbon X2 CrNi 19-11 1.4306 (TP)304L S30403C<0,03% CF-3 J92500
X2 CrNiN 18-10 1.4311 (TP)304LN S30453Medium carbon 302,304 S30400C > 0,03% X4 CrNi 18-10 1.4301 (TP)304 S30409
GX5 CrNi 19-10 1.4308 CF 8 J92600Ti-, Nb- X6 CrNiTi 18-10 1.4541 (TP)321 S32100stabilized (TP)321H S32109
X6 CrNiNb 18-10 1.4550 (TP)347 S34700(TP)347H S34709
GX5 CrNiNb 19-10 1.4552 CF-8C J92710
![Page 8: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/8.jpg)
Diameter (mm)Length (mm)Unit:Pieces / unit (nominal)Net weight/unit (kg)
Classification
Welding positions Current type
Chemical composition (w%), typical, all weld metal and ferritenumber
Mechanical properties, all weld metal
General description
Packaging, available sizes and identification
Identification Imprint: Tip colour:
Liability: All information in this data sheet is based on the best available knowledge, is subject to changewithout notice and can only be considered as suitable for general guidance.
Fumes: Consult information on Welding Safety Sheet, available upon request
Condition Yield strength Tensile strength Elongation Impact ISO-V(J)(N/mm2) (N/mm2) (%)
As weldedRequired AWS A5.4-92
EN 1600-97Typical values
ISO/ASME
Approvals
68
AWS A5.4-92 : E308L-15EN 1600-97 : E 19 9 L R 21
DB TÜV UDT+ + +
C Mn Si Cr Ni FN0.020 0.8 0.7 20.0 9.8 4-10
+20°C -20°C
not required min. 520 min. 35 not requiredmin. 320 min. 510 min. 30 not required
440 600 40 70 50
Grinox 56/308L-15 red
2.5 3.2300 300
box267 1894.0 4.2
MDS GRINOX 56 4
GRINOX 56
DC electr. +
PG/3G down
A rutile-basic stainless steel electrode for welding 304L or equivalent steelsSpecially developed for vertical down welding on DCRoot passes in grooves with root openingHigh corrosion resistance in oxidizing environments
8
0.2% Proof strength
Temperature rangepressure parts: -196...+350°Coxidation resistance: to 800°C
![Page 9: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/9.jpg)
Sizes Current Current Arc time Energy Dep.rate Weight/ Electrodes/ kg Electrodes/Diam. x length range type 1000 pcs. kg weldmetal kg weldmetal
(mm) (A) (s)* E(kJ) H(kg/h) (kg) B 1/N
Welding positions:Diameter(mm) Current(A)
Remarks
Welding parameters, optimum fill passes
Calculation data
Materials to be welded
- per electrode at max. current -
69
Steel grades EN 10088-1/-2 EN 102 13-4 W.Nr. ASTM/ACI UNSA240/A312/A351
Extra low carbon X2 CrNi 19-11 1.4306 (TP)304L S30403C<0,03% CF-3 J92500
X2 CrNiN 18-10 1.4311 (TP)304LN S30453Medium carbon 302,304 S30400C > 0,03% X4 CrNi 18-10 1.4301 (TP)304 S30409
GX5 CrNi 19-10 1.4308 CF 8 J92600Ti-, Nb- X6 CrNiTi 18-10 1.4541 (TP)321 S32100stabilized (TP)321H S32109
X6 CrNiNb 18-10 1.4550 (TP)347 S34700(TP)347H S34709
GX5 CrNiNb 19-10 1.4552 CF-8C J92710
GRINOX 56
2.5 x 300 60 - 70 DC+ 44 65 0.81 15.0 101 1.523.2 x 300 80 - 110 DC+ 51 117 1.2 23.5 59 1.39
* stub end = 35mm
3G down
2.5 703.2 100
![Page 10: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/10.jpg)
Diameter (mm)Length (mm)Unit:Pieces / unit (nominal)Net weight/unit (kg)
Classification
Welding positions Current type
Chemical composition (w%), typical, all weld metal and ferritenumber
Mechanical properties, all weld metal
General description
Packaging, available sizes and identification
Identification Imprint: Tip colour:
Liability: All information in this data sheet is based on the best available knowledge, is subject to changewithout notice and can only be considered as suitable for general guidance.
Fumes: Consult information on Welding Safety Sheet, available upon request
Condition Yield strength Tensile strength Elongation Impact ISO-V(J)(N/mm2) (N/mm2) (%)
As weldedRequired AWS A5.4-92
EN 1600-97Typical values
ISO/ASME
Approvals
70
Rutile-basic all position stainless steel electrodeFor Ti or Nb stabilized 304 or equivalent steelsExcellent resitance in oxidizing environments such as nitric acidHigh resistance to intergranular corrosionEasy slag release and smooth bead appearanceStrong electrode coatingWeldable on AC and DCAlso available in SRP (vacuum sealed)
AWS A5.4-92: E 347-16EN 1600-97 : E 19 9 Nb R 12
AC / DC electr. +/-
DB TÜV UDT + + +
C Mn Si Cr Ni Nb FN0.030 0.8 0.8 19.5 9.8 0.35 6-12
2.5 3.2 4.0 5.0350 350 350 450
Box186 105 73 523.9 3.7 3.9 5.2
MDS GRINOX 507 5
GRINOX 507/347-16 gold
GRINOX 507
pressure parts: -120...+400°Coxidation resistance: to 800°C
Temperature range
+20°C -20°C -60°C
not required min. 550 min. 25 not requiredmin. 350 min. 550 min. 25 not required
500 630 35 70 50 35
142536PA/1G PB/2F PC/2G PF/3G up PE/4G PF/5G up
0.2% Proof strength
![Page 11: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/11.jpg)
Sizes Current Current Arc time Energy Dep.rate Weight/ Electrodes/ kg Electrodes/Diam. x length range type 1000 pcs. kg weldmetal kg weldmetal
(mm) (A) (s)* E(kJ) H(kg/h) (kg) B 1/N
Welding positions:Diameter(mm) Current(A)
Remarks
Welding parameters, optimum fill passes
Calculation data
Materials to be welded
- per electrode at max. current -
71
2.5 x 350 40 - 75 DC+ 52 78 0.87 20.7 80 1.663.2 x 350 60 - 110 DC+ 54 119 1.4 34.9 48 1.674.0 x 350 80 - 150 DC+ 64 210 1.7 49.0 33 1.61
* stub end = 35mm
1G 2F 2G 3G 4G 5Gup
2.5 70 70 70 60 60 603.2 100 100 100 70 70 704.0 140 140 140 80
For rootpasses DC- is recommended.
GRINOX 507Steel grades EN 10088-1/-2 EN 102 13-4 W.Nr. ASTM/ACI UNS
A240/A312/A351Ti-, Nb X6 CrNiTi 18-10 1.4541 (TP)321 S32100stabilized (TP)321H S32109
X6 CrNiNb 18-10 1.4550 (TP)347 S34700(TP)347H S34709
GX5 CrNiNb 19-10 1.4552 CF-8C J92710
Non 302stabilized X4 CrNi 18-10 1.4301 (TP)304 S30400
X2 CrNi 19-11 1.4306 (TP)304L S30403GX5 CrNi 19-10 1.4308 CF-8 J92600
1.4312(TP)304H S30409
![Page 12: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/12.jpg)
Diameter (mm)Length (mm)Unit:Pieces / unit (nominal)Net weight/unit (kg)
Classification
Welding positions Current type
Chemical composition (w%), typical, all weld metal and ferritenumber
Mechanical properties, all weld metal
General description
Packaging, available sizes and identification
Identification Imprint: Tip colour:
Liability: All information in this data sheet is based on the best available knowledge, is subject to changewithout notice and can only be considered as suitable for general guidance.
Fumes: Consult information on Welding Safety Sheet, available upon request
Condition Yield strength Tensile strength Elongation Impact ISO-V(J)(N/mm2) (N/mm2) (%)
As weldedRequired AWS A5.4-92
EN 1600-97Typical values
ISO/ASME
Approvals
72
DC elec. +
GRINOX 506
C Mn Si Cr Ni Nb FN0.020 1.6 0.5 20.0 10.0 0.40 6-12
MDS GRINOX 506 3
3.2 4.0 5.0350 350 450
Box904.1
GRINOX 506 / 347-15 red
AWS A-5.4-92 : E 347-15EN 1600-97 : E 19 9 Nb B 22
DB TÜV UDT+ + +
Chemical composition (w%), typical, all weld metal and ferritenumber
+20°C -20°C
not required min. 520 min. 30 not requiredmin. 350 min. 550 min. 25 not required
500 630 35 80 50
Basic coated all position stainless steel electrodeFor Ti or Nb stabilized 304 or equivalent steelsExcellent resistance in oxidizing environments such as nitric acidHigh resistance to intergranular corrosionEasy slag release and smooth bead appearanceStrong electrode coating
PA/1G PB/2F PC/2G PF/3G up PE/4G PF/5G up142536
0.2% Proof strength
DC electr. +
Temperature rangepressure parts: -120...+400°Coxidation resistance: to 800°C
![Page 13: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/13.jpg)
Sizes Current Current Arc time Energy Dep.rate Weight/ Electrodes/ kg Electrodes/Diam. x length range type 1000 pcs. kg weldmetal kg weldmetal
(mm) (A) (s)* E(kJ) H(kg/h) (kg) B 1/N
Welding positions:Diameter(mm) Current(A)
Remarks
Welding parameters, optimum fill passes
Calculation data
Materials to be welded
- per electrode at max. current -
73
GRINOX 506
3.2 x 350 80 - 100 DC+ 51 135 1.3 32.4 53 1.724.0 x 350 100 - 130 DC+ 66 206 1.7 44.4 32 1.565.0 x 450 130 - 160 DC+ 69 378 2.3 90.9 23 1.92
* stub end = 35mm
1G 2F 2G 3G 4G 5Gup up
3.2 95 90 90 75 75 754.0 125 110 125 100 100 1005.0 150 150
Steel grades EN 10088-1/-2 EN 102 13-4 W.Nr. ASTM/ACI UNSA240/A312/A351
Ti-, Nb X6 CrNiTi 18-10 1.4541 (TP)321 S32100stabilized (TP)321H S32109
X6 CrNiNb 18-10 1.4550 (TP)347 S34700(TP)347H S34709
GX5 CrNiNb 19-10 1.4552 CF-8C J92710
Non 302stabilized X4 CrNi 18-10 1.4301 (TP)304 S30400
X2 CrNi 19-11 1.4306 (TP)304L S30403GX5 CrNi 19-10 1.4308 CF-8 J92600
1.4312(TP)304H S30409
![Page 14: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/14.jpg)
Diameter (mm)Length (mm)Unit:Pieces / unit (nominal)Net weight/unit (kg)
Classification
Welding positions Current type
Chemical composition (w%), typical, all weld metal and ferritenumber
Mechanical properties, all weld metal
General description
Packaging, available sizes and identification
Identification Imprint: Tip colour:
Liability: All information in this data sheet is based on the best available knowledge, is subject to changewithout notice and can only be considered as suitable for general guidance.
Fumes: Consult information on Welding Safety Sheet, available upon request
Condition Yield strength Tensile strength Elongation Impact ISO-V(J)(N/mm2) (N/mm2) (%)
As weldedRequired AWS A5.4-92
EN 1600-97Typical values
ISO/ASME
Approvals
74
AWS A 5.4-92 : E 316 L-16EN 1600-97 : E 19 12 3 L R 32
AC/DC electr. +/-
2.0 2.5 3.2 4.0 5.0300 350 350 350 350
box300 230 115 68 493.2 4.8 3.7 3.6 3.8
MDS GRINOX 210 3
GRINOX 210
C Mn Si Cr Ni Mo FN0.020 0.8 0.8 18.0 11.5 2.85 4-10
GRINOX 210 / 316L-16 red
UDT+
Rutile-basic all position stainless steel electrode for 316L or equivalent steelsMolybdenum level min. 2.7%High resistance to general and intergranular corrosionSmooth weld appearanceEasy slag releaseStrong electrode coatingWeldable on AC and DC
Chemical composition (w%), typical, all weld metal
PA/1G PB/2F PC/2G PF/3G up PE/4G14253
0.2% Proof strength+20°C -120°C
not required min. 490 min. 30 not requiredmin. 320 min. 510 min. 25 not required
450 580 39 60 40
Temperature rangepressure parts: -120...+350°Coxidation resistance: n.a.
![Page 15: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/15.jpg)
Sizes Current Current Arc time Energy Dep.rate Weight/ Electrodes/ kg Electrodes/Diam. x length range type 1000 pcs. kg weldmetal kg weldmetal
(mm) (A) (s)* E(kJ) H(kg/h) (kg) B 1/N
Welding positions:Diameter(mm) Current(A)
Remarks
Welding parameters, optimum fill passes
Calculation data
Materials to be welded
- per electrode at max. current -
75
GRINOX 210
Steel grades EN 10088-1/-2 EN 102 13-4 W.Nr. ASTM/ACI UNSA240/A312/A351
Extra low carbon X2 CrNiMo 17-12-2 1.4404 (TP)316L S31603C<0,03% CF-3M J92800
X2 CrNiMo 18-14-3 1.4435 (TP)316L S31603X2 CrNiMoN 17-11-2 1.4406 (TP)316LN S31653X2 CrNiMoN 17-13-3 1.4429
Medium carbon X4 CrNiMo 17-12-2 1.4401 (TP)316 S31600C > 0,03% X4 CrNiMo 17-13-3 1.4436
GX5 CrNiMo 19-11 1.4408 CF 8M J92900Ti-, Nb X6 CrNiMoTi 17-12-2 1.4571 316Ti S31635stabilized X6 CrNiMoNb 17-12-2 1.4580 316CbS31640
X6 CrNiNb 18-10 1.4550 (TP)347 S34700GX5 CrNiNb 19-10 1.4552 CF-8C J92710
2.0 x 300 40 - 502.5 x 350 55 - 753.2 x 350 70 - 1104.0 x 350 100 - 1405.0 x 450 140 - 190
1G 2F 2G 3G 4G 5Gup up
2.0 45 45 40 40 402.5 70 70 70 60 60 603.2 100 100 100 70 70 704.0 140 140 140 805.0 180 180 180
For rootpasses DC- is recommended.
Sizes Current Current Arc time Energy Dep.rate Weight/ Electrodes/ kg Electrodes/Diam. x length range type - per electrode at max. current - 1000 pcs. kg weldmetal kg weldmetal
(mm) (A) (s)* E(kJ) H(kg/h) (kg) B 1/N
![Page 16: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/16.jpg)
Diameter (mm)Length (mm)Unit:Pieces / unit (nominal)Net weight/unit (kg)
Classification
Welding positions Current type
Chemical composition (w%), typical, all weld metal and ferritenumber
Mechanical properties, all weld metal
General description
Packaging, available sizes and identification
Identification Imprint: Tip colour:
Liability: All information in this data sheet is based on the best available knowledge, is subject to changewithout notice and can only be considered as suitable for general guidance.
Fumes: Consult information on Welding Safety Sheet, available upon request
Condition Yield strength Tensile strength Elongation Impact ISO-V(J)(N/mm2) (N/mm2) (%)
As weldedRequired AWS A5.4-92
EN 1600-97Typical values
ISO/ASME
Approvals
76
A rutile-basic all position stainless steel electrode for 316L or equivalent steelsMolybdenum level min. 2.7%Mirror like bead appearanceSelf releasing slagGood side wall fusion, no undercutHigh resistance to porosityWeldable on AC and DC+ polarity
AWS A5.4-92 : E316L-16*EN 1600-97 : E 19 12 3 LR 12 * deviations see remarks
AC / DC electr. +
DB TÜV UDT+ + +
C Mn Si Cr Ni Mo FN0.020 0.8 1.0 18.0 11.5 2.8 4-10
+20°C -20°C -105°C
not required min. 490 min. 30 not requiredmin. 320 min. 510 min. 25 not required
450 580 40 70 60 40
1.6 2.0 2.5 3.2 4.0 4.0 5.0250 300 350 350 350 450 450
Box435 278 180 110 68 68 412.7 3.2 3.8 3.8 3.6 4.7 4.4
MDS GRINOX 510 2
GRINOX 510/316L-16 red
GRINOX 510
142536PA/1G PB/2F PC/2G PF/3G up PE/4G PF/5G up
0.2% Proof strength
![Page 17: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/17.jpg)
Sizes Current Current Arc time Energy Dep.rate Weight/ Electrodes/ kg Electrodes/Diam. x length range type 1000 pcs. kg weldmetal kg weldmetal
(mm) (A) (s)* E(kJ) H(kg/h) (kg) B 1/N
Welding positions:Diameter(mm) Current(A)
Remarks
Welding parameters, optimum fill passes
Calculation data
Materials to be welded
- per electrode at max. current -
77
GRINOX 510Steel grades EN 10088-1/-2 EN 102 13-4 W.Nr. ASTM/ACI UNS
A240/A312/A351Extra low carbon X2 CrNiMo 17-12-2 1.4404 (TP)316L S31603C<0,03% CF-3M J92800
X2 CrNiMo 18-14-3 1.4435 (TP)316L S31603X2 CrNiMoN 17-11-2 1.4406 (TP)316LN S31653X2 CrNiMoN 17-13-3 1.4429
Medium carbon X4 CrNiMo 17-12-2 1.4401 (TP)316 S31600C > 0,03% X4 CrNiMo 17-13-3 1.4436
GX5 CrNiMo 19-11 1.4408 CF 8M J92900Ti-, Nb X6 CrNiMoTi 17-12-2 1.4571 316Ti S31635stabilized X6 CrNiMoNb 17-12-2 1.4580 316CbS31640
X6 CrNiNb 18-10 1.4550 (TP)347 S34700GX5 CrNiNb 19-10 1.4552 CF-8C J92710
1.5 x 250 20 - 402.0 x 300 35 - 50 DC+ 39 49 0.59 11.4 155 1.792.5 x 350 45 - 80 DC+ 46 92 0.95 21.5 83 1.793.2 x 350 80 - 115 DC+ 51 157 1.5 35.3 48 1.694.0 x 450 100 - 155 DC+ 75 339 1.9 69.2 24 1.695.0 x 450 150 - 220 DC+ 85 577 2.7 107.8 16 1.69
* stub end = 35mm
1G 2F 2G 3G 4G 5Gup up
2.0 45 45 40 40 402.5 70 70 70 60 60 603.2 100 100 100 70 70 704.0 140 140 1405.0 180 180
For rootpasses DC- is recommended.
Deviation: Chemical composition: Si max. 1.2%; AWS A5.4-92: max. 0.90%
![Page 18: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/18.jpg)
Diameter (mm)Length (mm)Unit:Pieces / unit (nominal)Net weight/unit (kg)
Classification
Welding positions Current type
Chemical composition (w%), typical, all weld metal and ferritenumber
Mechanical properties, all weld metal
General description
Packaging, available sizes and identification
Identification Imprint: Tip colour:
Liability: All information in this data sheet is based on the best available knowledge, is subject to changewithout notice and can only be considered as suitable for general guidance.
Fumes: Consult information on Welding Safety Sheet, available upon request
Condition Yield strength Tensile strength Elongation Impact ISO-V(J)(N/mm2) (N/mm2) (%)
As weldedRequired AWS A5.4-92
EN 1600-97Typical values
ISO/ASME
Approvals
78
AWS A-5.4-92 : E316 L-15EN 1600-97 : E19 12 3 L B 22
DC electr. +
GRINOX 9
C Mn Si Cr Ni Mo FN0.025 1.6 0.4 18.5 11.0 2.7 4-10
MDS GRINOX 9 3
GRINOX 9 / 316L-15 red
2.5 3.2 4.0 5.0350 350 350 450
Box191 126 87 663.8 4.0 4.1 5.3
TÜV UDT+ +
Basic coated electrode for low temperature applicationsGood impact properties down to -196°CGood weldability and smooth bead appearanceLow carbon contentService temperature up to 400°CHigh resistance against general and intercristallinecorrosion
PA/1G PB/2F PC/2G PF/3G up PG/3G down PE/4G
Chemical composition (w%), typical, all weld metal and ferritenumber
+20° -196°
not required min. 490 min. 30 not requiredmin. 320 min. 510 min. 25 not required
450 650 35 100 35
142583
0.2% Proof strength
Temperature rangepressure parts: -120...+350°Coxidation resistance: n.a.
![Page 19: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/19.jpg)
Sizes Current Current Arc time Energy Dep.rate Weight/ Electrodes/ kg Electrodes/Diam. x length range type 1000 pcs. kg weldmetal kg weldmetal
(mm) (A) (s)* E(kJ) H(kg/h) (kg) B 1/N
Welding positions:Diameter(mm) Current(A)
Remarks
Welding parameters, optimum fill passes
Calculation data
Materials to be welded
- per electrode at max. current -
79
GRINOX 9
2.5 x 350 50 - 70 DC+ 50 86 0.82 19.2 88 1.893.2 x 350 60 - 90 DC+ 51 135 1.3 31.3 53 1.724.0 x 350 80 - 120 DC+ 66 206 1.7 47.6 32 1.56
* stub end = 35mm
1G 2F 2G 3G 4G 5Gup up
2.5 60 60 60 60 60 603.2 95 90 90 75 75 754.0 125 110 125 100 100 100
Steel grades EN 10088-1/-2 EN 102 13-4 W.Nr. ASTM/ACI UNSA240/A312/A351
Extra low carbon X2 CrNiMo 17-12-2 1.4404 (TP)316L S31603C<0,03% CF-3M J92800
X2 CrNiMo 18-14-3 1.4435 (TP)316L S31603X2 CrNiMoN 17-11-2 1.4406 (TP)316LN S31653X2 CrNiMoN 17-13-3 1.4429
Medium carbon X4 CrNiMo 17-12-2 1.4401 (TP)316 S31600C > 0,03% X4 CrNiMo 17-13-3 1.4436
GX5 CrNiMo 19-11 1.4408 CF 8M J92900Ti-, Nb X6 CrNiMoTi 17-12-2 1.4571 316Ti S31635stabilized X6 CrNiMoNb 17-12-2 1.4580 316Cb S31640
X6 CrNiNb 18-10 1.4550 (TP)347 S34700GX5 CrNiNb 19-10 1.4552 CF-8C J92710
![Page 20: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/20.jpg)
Diameter (mm)Length (mm)Unit:Pieces / unit (nominal)Net weight/unit (kg)
Classification
Welding positions Current type
Chemical composition (w%), typical, all weld metal and ferritenumber
Mechanical properties, all weld metal
General description
Packaging, available sizes and identification
Identification Imprint: Tip colour:
Liability: All information in this data sheet is based on the best available knowledge, is subject to changewithout notice and can only be considered as suitable for general guidance.
Fumes: Consult information on Welding Safety Sheet, available upon request
Condition Yield strength Tensile strength Elongation Impact ISO-V(J)(N/mm2) (N/mm2) (%)
As weldedRequired AWS A5.4-92
EN 1600-97Typical values
ISO/ASME
Approvals
80
GRINOX 57
AWS A5.4-92 : E316L-15EN 1600-97 : 19 12 3 L R 21
AC/DC electr. +
DB GL TÜV UDT+ 4429 + +
C Mn Si Cr Ni Mo FN0.020 0.7 0.85 18.0 11.5 2.8 4-10
+20°C -20°C
not required min. 490 min. 30 not requiredmin. 320 min. 510 min. 25 not required
500 620 35 50 45
2.5 3.2300 300
box250 1893.8 4.2
Grinox 57 / 316L-15 red
MDS GRINOX 3
PG/3G down
A rutile-basic stainless steel electrode for welding 316L or equivalent steelsMolybdenum level min. 2.7%Specially developed for vertical down welding on DCRoot passes in grooves with root openingHigh general corrosion resistance
8
Temperature rangepressure parts: -60...+400°Coxidation resistance: n.a.
0.2% Proof strength
![Page 21: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/21.jpg)
Sizes Current Current Arc time Energy Dep.rate Weight/ Electrodes/ kg Electrodes/Diam. x length range type 1000 pcs. kg weldmetal kg weldmetal
(mm) (A) (s)* E(kJ) H(kg/h) (kg) B 1/N
Welding positions:Diameter(mm) Current(A)
Remarks
Welding parameters, optimum fill passes
Calculation data
Materials to be welded
- per electrode at max. current -
81
GRINOX 57
Steel grades EN 10088-1/-2 EN 102 13-4 W.Nr. ASTM/ACI UNSA240/A312/A351
Extra low carbon X2 CrNiMo 17-12-2 1.4404 (TP)316L S31603C<0,03% CF-3M J92800
X2 CrNiMo 18-14-3 1.4435 (TP)316L S31603X2 CrNiMoN 17-11-2 1.4406 (TP)316LN S31653X2 CrNiMoN 17-13-3 1.4429
Medium carbon X4 CrNiMo 17-12-2 1.4401 (TP)316 S31600C > 0,03% X4 CrNiMo 17-13-3 1.4436
GX5 CrNiMo 19-11 1.4408 CF 8M J92900Ti-, Nb X6 CrNiMoTi 17-12-2 1.4571 316Ti S31635stabilized X6 CrNiMoNb 17-12-2 1.4580 316Cb S31640
X6 CrNiNb 18-10 1.4550 (TP)347 S34700GX5 CrNiNb 19-10 1.4552 CF-8C J92710
2.5 x 300 60 - 70 DC+ 44 71 0.83 14.9 98 1.473.2 x 300 80 - 110 DC+ 47 118 1.3 23.9 59 1.41
* stub end = 35mm
3G (down)
2.5 703.2 100
![Page 22: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/22.jpg)
Diameter (mm)Length (mm)Unit:Pieces / unit (nominal)Net weight/unit (kg)
Classification
Welding positions Current type
Chemical composition (w%), typical, all weld metal and ferritenumber
Mechanical properties, all weld metal
General description
Packaging, available sizes and identification
Identification Imprint: Tip colour:
Liability: All information in this data sheet is based on the best available knowledge, is subject to changewithout notice and can only be considered as suitable for general guidance.
Fumes: Consult information on Welding Safety Sheet, available upon request
Condition Yield strength Tensile strength Elongation Impact ISO-V(J)(N/mm2) (N/mm2) (%)
As weldedRequired AWS A5.4-92
EN 1600-97Typical values
ISO/ASME
Approvals
82
DC electr. +
DB TÜV UDT+ + +
GRINOX 513
C Mn Si Cr Ni Mo Nb FN0.025 1.5 0.4 18.0 11.0 2.7 0.5 6-12
MDS GRINOX 513 3
2.5 3.2 4.0350 350 350
Box191 121 913.8 3.9 4.2
AWS A5.4-92 : E318-15*EN 1600-97 : E 19 12 3 Nb B 22
* for deviations see remarks
GRINOX 513 / 318-15 red
Chemical composition (w%), typical, all weld metal and ferritenumber
PA/1G PB/2F PC/2G PF/3G up PE/4G PF/5G up
+20°C
not required min. 550 min. 25 not requiredmin. 350 min. 550 min. 25 not required
430 650 30 90
Basic all position stainless steel electrodes for weldingTi or Nb stabilized 316 or equivalent steelsHigh resistance to general and intergranular corrosionSmooth bead appearanceEasy slag releaseStrong electrode coatingSpecially developed for highly restrained structures
142536
0.2% Proof strength
![Page 23: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/23.jpg)
Sizes Current Current Arc time Energy Dep.rate Weight/ Electrodes/ kg Electrodes/Diam. x length range type 1000 pcs. kg weldmetal kg weldmetal
(mm) (A) (s)* E(kJ) H(kg/h) (kg) B 1/N
Welding positions:Diameter(mm) Current(A)
Remarks
Welding parameters, optimum fill passes
Calculation data
Materials to be welded
- per electrode at max. current -
83
GRINOX 513
2.5 x 350 50 - 70 DC+ 50 86 0.82 17.6 88 1.893.2 x 350 80 - 100 DC+ 51 135 1.3 28.5 53 1.724.0 x 350 100 - 130 DC+ 66 206 1.7 43.8 32 1.56
1G 2F 2G 3G 4G 5Gup
2.5 60 60 60 60 60 603.2 95 90 90 75 75 754.0 125 110 125 100 100 100
Deviation chemical compositionNi = 10.0-13.0; AWS Ni = 11.0-14.0
Steel grades EN 10088-1/-2 EN 102 13-4 W.Nr. ASTM/ACI UNSA240/A312/A351
Extra low carbon X2 CrNiMo 17-12-2 1.4404 (TP)316L S31603C<0,03% CF-3M J92800
X2 CrNiMo 18-14-3 1.4435 (TP)316L S31603X2 CrNiMoN 17-11-2 1.4406 (TP)316LN S31653X2 CrNiMoN 17-13-3 1.4429
Medium carbon X4 CrNiMo 17-12-2 1.4401 (TP)316 S31600C > 0,03% X4 CrNiMo 17-13-3 1.4436
GX5 CrNiMo 19-11 1.4408 CF 8M J92900Ti-, Nb X6 CrNiMoTi 17-12-2 1.4571 316Ti S31635stabilized X6 CrNiMoNb 17-12-2 1.4580 316Cb S31640
X6 CrNiNb 18-10 1.4550 (TP)347 S34700GX5 CrNiNb 19-10 1.4552 CF-8C J92710
![Page 24: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/24.jpg)
Diameter (mm)Length (mm)Unit:Pieces / unit (nominal)Net weight/unit (kg)
Classification
Welding positions Current type
Chemical composition (w%), typical, all weld metal and ferritenumber
Mechanical properties, all weld metal
General description
Packaging, available sizes and identification
Identification Imprint: Tip colour:
Liability: All information in this data sheet is based on the best available knowledge, is subject to changewithout notice and can only be considered as suitable for general guidance.
Fumes: Consult information on Welding Safety Sheet, available upon request
Condition Yield strength Tensile strength Elongation Impact ISO-V(J)(N/mm2) (N/mm2) (%)
As weldedRequired AWS A5.4-92
EN 1600-97Typical values
ISO/ASME
Approvals
84
AWS A5.4-92: E318-16EN 1600-97 : E 19 12 3 Nb R 12
AC / DC electr. +/-
DB TÜV UDT+ + +
C Mn Si Cr Ni Mo Nb FN0.030 0.8 0.85 18.0 11.5 2.7 0.35 6-12
2.0 2.5 2.5 3.2 4.0 4.0 5.0300 250 350 350 350 450 450
Box300 173 173 105 68 68 493.2 2.6 3.8 3.8 3.6 4.7 5.0
MDS GRINOX 514 3
Rutile basic-all position stainless steel electrodes for weldingTi or Nb stabilized 316 or equivalent steelsHigh resistance to general and intergranular corrosionSmooth bead appearanceEasy slag releaseStrong electrode coatingWeldable on AC and DCAlso available in SRP (vacuum sealed)
GRINOX 514 red
GRINOX 514
Temperature rangepressure parts : -60...+400°Coxidation resistance : n.a.
142536PA/1G PB/2F PC/2G PF/3G up PE/4G PF/5G up
0.2% Proof strength+20°C -20°C -60°C
not required min. 550 min. 25 not requiredmin. 350 min. 550 min. 25 not required
500 630 38 60 50 35
![Page 25: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/25.jpg)
Sizes Current Current Arc time Energy Dep.rate Weight/ Electrodes/ kg Electrodes/Diam. x length range type 1000 pcs. kg weldmetal kg weldmetal
(mm) (A) (s)* E(kJ) H(kg/h) (kg) B 1/N
Welding positions:Diameter(mm) Current(A)
Remarks
Welding parameters, optimum fill passes
Calculation data
Materials to be welded
- per electrode at max. current -
85
Steel grades EN 10088-1/-2 EN 102 13-4 W.Nr. ASTM/ACI UNSA240/A312/A351
Extra low carbon X2 CrNiMo 17-12-2 1.4404 (TP)316L S31603C<0,03% CF-3M J92800
X2 CrNiMo 18-14-3 1.4435 (TP)316L S31603X2 CrNiMoN 17-11-2 1.4406 (TP)316LN S31653
X2 CrNiMoN 17-13-3 1.4429Medium carbon X4 CrNiMo 17-12-2 1.4401 (TP)316 S31600C > 0,03% X4 CrNiMo 17-13-3 1.4436
GX5 CrNiMo 19-11 1.4408 CF 8M J92900Ti-, Nb X6 CrNiMoTi 17-12-2 1.4571 316Ti S31635stabilized X6 CrNiMoNb 17-12-2 1.4580 316Cb S31640
X6 CrNiNb 18-10 1.4550 (TP)347 S34700GX5 CrNiNb 19-10 1.4552 CF-8C J92710
2.0 x 300 30 - 60 DC+ 36 36 0.65 10.7 152 1.642.5 x 250 40 - 902.5 x 350 40 - 90 DC+ 46 82 0.98 20.3 80 1.643.2 x 350 70 - 110 DC+ 52 137 1.4 32.1 48 1.544.0 x 350 90 - 140 DC+ 61 212 1.9 48.6 31 1.494.0 x 450 90 - 1405.0 x 450 140 - 190
* stub end = 35 mm
1G 2F 2G 3G 4G 5Gup up
2.0 45 45 40 40 402.5 70 70 70 60 60 603.2 100 100 100 70 70 704.0 140 140 140 805.0
For rootpasses DC- is recommended.
GRINOX 514
![Page 26: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/26.jpg)
Diameter (mm)Length (mm)Unit:Pieces / unit (nominal)Net weight/unit (kg)
Classification
Welding positions Current type
Chemical composition (w%), typical, all weld metal and ferritenumber
Mechanical properties, all weld metal
General description
Packaging, available sizes and identification
Identification Imprint: Tip colour:
Liability: All information in this data sheet is based on the best available knowledge, is subject to changewithout notice and can only be considered as suitable for general guidance.
Fumes: Consult information on Welding Safety Sheet, available upon request
Condition Yield strength Tensile strength Elongation Impact ISO-V(J)(N/mm2) (N/mm2) (%)
As weldedRequired AWS A5.4-92
EN 1600-97Typical values
ISO/ASME
Approvals
86
EN 1600-97 : E 18 16 5 N L R 32
AC / DC electr. +/-
GL TÜV UDT 4439 + +
C Mn Si Cr Ni Mo N FN0.020 1.3 0.8 18.0 17.0 4.6 0.18 <0.3
2.5 3.2 4.0350 350 350
Box174 115 824.0 3.9 4.3
MDS GRINOX 36 4
GRINOX 36 red
GRINOX 36
Rutile-basic fully austenitic 4.5% Mo-containing stainless steel electrodeElectrode for welding AISI 317LN or equivalent stainless steelsHigh resistance to - pitting corrosion
- intergranular corrosion- stress corrosion
Good impact toughness at low temperatureEasy slag release and good weld appearance
Chemical composition (w%), typical, all weld metal and ferritenumber
142536PA/1G PB/2F PC/2G PF/3G up PE/4G PF/5G up
+20°C -20°C -196°CAs weldedRequired: EN 1600-97 min. 300 min. 480 min. 25 not requiredTypical values 460 650 40 70 70 50
Temperature rangepressure parts: -120...+400°Coxidation resistance: n.a.
![Page 27: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/27.jpg)
Sizes Current Current Arc time Energy Dep.rate Weight/ Electrodes/ kg Electrodes/Diam. x length range type 1000 pcs. kg weldmetal kg weldmetal
(mm) (A) (s)* E(kJ) H(kg/h) (kg) B 1/N
Welding positions:Diameter(mm) Current(A)
Remarks
Welding parameters, optimum fill passes
Calculation data
Materials to be welded
- per electrode at max. current -
87
2.5 x 350 40 - 75 DC+ 78 153 0.58 19.8 79 1.563.2 x 350 60 - 110 DC+ 55 152 1.3 33.8 49 1.674.0 x 350 90 - 145 DC+ 67 291 1.8 51.6 29 1.47
* stub end= 35mm
1G 2F 2G 3G 4G 5Gup up
2.5 70 70 70 60 60 603.2 100 90 100 65 65 654.0 130 125 130 80
.For rootpasses DC- is recommended.
GRINOX 36
Steel grades EN 10088-1/-2 EN 102 13-4 W.Nr. ASTM/ACI UNSFully X2 CrNiMoN 17-11-2 1.4406 (TP)316LN S31653austenitic X2 CrNiMoN 17-13-3 1.4429 (TP)316LN S31653CrNiMo- X2 CrNiMo 18-14-3 1.4435 (TP)316L S31603corrosion X2 CrNiMo 18-15-4 1.4438 317L S31725resistant steel X2 CrNiMoN 17-13-5 1.4439 317LN S31726
G-X2 CrNiMoN 17-13-4 GX2 CrNiMo 17-13-41.4446G-X6 CrNiMo 17-13 GX6 CrNiMo 17-13 1.4448
![Page 28: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/28.jpg)
Diameter (mm)Length (mm)Unit:Pieces / unit (nominal)Net weight/unit (kg)
Classification
Welding positions Current type
Chemical composition (w%), typical, all weld metal and ferritenumber
Mechanical properties, all weld metal
General description
Packaging, available sizes and identification
Identification Imprint: Tip colour:
Liability: All information in this data sheet is based on the best available knowledge, is subject to changewithout notice and can only be considered as suitable for general guidance.
Fumes: Consult information on Welding Safety Sheet, available upon request
Condition Yield strength Tensile strength Elongation Impact ISO-V(J)(N/mm2) (N/mm2) (%)
As weldedRequired AWS A5.4-92
EN 1600-97Typical values
ISO/ASME
Approvals
88
GRINOX 51
EN 1600-97 : E 20 16 3 Mn N L B 22
DC electr. +
C Mn Si Cr Ni Mo N0.030 7.3 0.4 20.0 16.0 3.0 0.16
2.5 3.2 4.0 5.0350 350 350 450
Box211 138 93 593.9 4.1 4.3 5.4
GRINOX 51 red
MDS GRINOX 51 5
Basic coated electrode for fully austenitic CrNiMo-steelsService temperature from -269°C to 350°CCryogenic austenitic stainless steelsCryogenic nickel steels and their joiningNon magnetic stainless steels
UDT+
PA/1G PB/2F PC/2G PF/3G up PE/4G PF/5G up142536
0.2% Proof strength+20°C -196°C
EN 1600-97 min. 320 min. 510 min. 25 not requiredTypical values 460 650 35 80 50
Temperature rangepressurized: -269 ... +350°Cscaling resistance: n.a.
![Page 29: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/29.jpg)
Sizes Current Current Arc time Energy Dep.rate Weight/ Electrodes/ kg Electrodes/Diam. x length range type 1000 pcs. kg weldmetal kg weldmetal
(mm) (A) (s)* E(kJ) H(kg/h) (kg) B 1/N
Welding positions:Diameter(mm) Current(A)
Remarks
Welding parameters, optimum fill passes
Calculation data
Materials to be welded
- per electrode at max. current -
89
GRINOX 51
2.5 x 350 45 - 70 DC+ 44 71 0.96 19.0 85 1.523.2 x 350 70 - 105 DC+ 53 132 1.4 31.0 48 1.394.0 x 450 100 - 130 DC+ 86 264 1.7 47.6 25 1.415.0 x 450 120 - 155 DC+ 82 388 2.7 92.8 16 1.39
* stub end = 35mm
1G 2F 2G 3G 4G 5Gup up
2.5 60 60 60 60 60 603.2 90 90 90 704.0 140 115 130 955.0 160 165
Steel grades W.Nr. ASTM/ACI UNSEN 10088-1/-2 Austenitic X2 CrNiN 18-10 1.4311 (TP)304LN S30453
nitrogen alloyed X2 CrNiMoN 17-11-2 1.4406 (TP)316LN S31653CrNi-and X2 CrNiMoN 17-13-3 1.4429
CrNiMo-steel X2 CrNiMoN 17-13-5 1.4439 317LN S31726
SEW 390 Austenitic X2 CrNiMoN 22-15 1.3951A-magnetic X2 CrNiMoN18-14-3 1.3952steel X2 CrNiMo 18-15 1.3953
X8 CrMnNi 18-8 1.3965
SEW 685 Steel for GX6 CrNi 18-10 1.6902low temperature GX5 CrNiNb 18-10 1.6905
EN 10028-4 12 Ni 14 1.5637X12 Ni 5 1.5680
![Page 30: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/30.jpg)
Diameter (mm)Length (mm)Unit:Pieces / unit (nominal)Net weight/unit (kg)
Classification
Welding positions Current type
Chemical composition (w%), typical, all weld metal and ferritenumber
Mechanical properties, all weld metal
General description
Packaging, available sizes and identification
Identification Imprint: Tip colour:
Liability: All information in this data sheet is based on the best available knowledge, is subject to changewithout notice and can only be considered as suitable for general guidance.
Fumes: Consult information on Welding Safety Sheet, available upon request
Condition Yield strength Tensile strength Elongation Impact ISO-V(J)(N/mm2) (N/mm2) (%)
As weldedRequired AWS A5.4-92
EN 1600-97Typical values
ISO/ASME
Approvals
90
AWS A5.4-92 : E 310Mo-15*
DC electr. +
TÜV UDT+ +
MDS GRINOX 67 4
2.5 3.2 4.0350 350 350
Box180 125 823.7 4.0 4.0
GRINOX 67 / 310 Mo-15 red
EN 1600-97 : E 25 22 2 N L B 22** Deviations see remarks
GRINOX 67
A basic high CrNiMo-alloyed fully austenitic all position electrodeExcellent corrosion resistance in strong oxydizing and slightly reducing mediaEspecially developed for urea and nitrid acid plantsHigh resistance to intergranular corrosionExcellent performance in the Huey-testWeldable on DC+ polarity
Chemical composition (w%), typical, all weld metal and ferritenumber
+20°C -196°C
not required min. 550 min. 30 not requiredmin. 320 min. 510 min. 25 not required
440 620 35 90 50
C Mn Si Cr Ni Mo N FN0.03 4.5 0.4 25.0 22.0 2.2 0.13 0.6
PA/1G PB/2F PC/2G PF/3G up PE/4G PF/5G up142536
0.2% Proof strength
Temperature rangepressurized: -40 ...+400°Cscaling resistance: n.a.
![Page 31: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/31.jpg)
Sizes Current Current Arc time Energy Dep.rate Weight/ Electrodes/ kg Electrodes/Diam. x length range type 1000 pcs. kg weldmetal kg weldmetal
(mm) (A) (s)* E(kJ) H(kg/h) (kg) B 1/N
Welding positions:Diameter(mm) Current(A)
Remarks
Welding parameters, optimum fill passes
Calculation data
Materials to be welded
- per electrode at max. current -
91
Steel grades DIN W.Nr. AFNOR ASTM / ACI SIS UNSFully X1 CrNiMoN 25 25 2 1.4465austenitic X3 CrNiMoTi 25 25 1.4577corrosion X2 CrNi 19 11 1.4306 Z2 CN 18.10 (TP)304L 2352 S30403resistent CF-3 J92500CrNiMo-steel X2 CrNiN 18 10 1.4311 Z2 CN 18.10 à 1'N (TP)304LN S30453
310S S31008
Also very well applicable for build-up welding on low alloyed steel, such as pipe platesBufferlayer in applications from -196 to +350°C
2.5 x 350 50 - 75 DC+ 50 86 0.82 21.5 88 1.893.2 x 350 70 - 105 DC+ 51 135 1.3 32.5 53 1.724.0 x 350 100 - 135 DC+ 66 206 1.7 48.5 32 1.56
* stub end = 35mm
1G 2F 2G 3G 4G 5Gup up
2.5 60 60 60 60 60 603.2 95 90 90 75 75 754.0 125 110 125 100 100 100
Deviation: Chemical composition - welding with heat input max. 1.5 kJ/mmCr = 24.5 - 26.0%; AWS A5.4-92: Cr = 25.0 - 28.0% - interpass temperature max. 150°CNi = 21.5 - 22.5%; AWS A5.4-92: Ni = 20.0 - 22.0%Mn = 4.5-5.3%; AWS A5.4-92; Mn = 1.0-2.5%;EN 1600-97: Mn = 1.0 - 5.0%
GRINOX 67
Application advice
![Page 32: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/32.jpg)
Diameter (mm)Length (mm)Unit:Pieces / unit (nominal)Net weight/unit (kg)
Classification
Welding positions Current type
Chemical composition (w%), typical, all weld metal and ferritenumber
Mechanical properties, all weld metal
General description
Packaging, available sizes and identification
Identification Imprint: Tip colour:
Liability: All information in this data sheet is based on the best available knowledge, is subject to changewithout notice and can only be considered as suitable for general guidance.
Fumes: Consult information on Welding Safety Sheet, available upon request
Condition Yield strength Tensile strength Elongation Impact ISO-V(J)(N/mm2) (N/mm2) (%)
As weldedRequired AWS A5.4-92
EN 1600-97Typical values
ISO/ASME
Approvals
92
AWS A5.4-92 : E 385-16*EN 1600-97 : E 20 25 5 Cu NL R 12 * Deviations see remarks
DC electr. +
TÜV UDT+ +
C Mn Si Cr Ni Mo Cu0.02 1.2 0.9 20.0 25.0 5.0 1.5
2.5 3.2 4.0350 350 350
box200 124 853.9 3.9 4.0
Grinox 65/385-16 red
MDS Grinox 65 4
+20°C -10°C
not required min. 520 min. 30 not requiredmin. 320 min. 510 min. 25 not required
410 620 40 80 100
A rutile-basic fully austenitic all position electrodeSmooth bead appearanceEasy slag releaseEspecially developed for applications in:- phosphoric acid and sulphuric acid- paper mill equipmentWorld wide reputation for reliabilityWeldable on DC+ polarity
GRINOX 65
Current type
Temperature rangepressurized:-10 ...+400°Cscaling resistance: n.a.
PA/1G PB/2F PC/2G PF/3G up PE/4G PF/5G up142536
![Page 33: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/33.jpg)
Sizes Current Current Arc time Energy Dep.rate Weight/ Electrodes/ kg Electrodes/Diam. x length range type 1000 pcs. kg weldmetal kg weldmetal
(mm) (A) (s)* E(kJ) H(kg/h) (kg) B 1/N
Welding positions:Diameter(mm) Current(A)
Remarks
Welding parameters, optimum fill passes
Calculation data
Materials to be welded
- per electrode at max. current -
93
Steel grades EN 10088-1/-2 EN 102 13-4 W.Nr.Fully austenitic GX7 NiCrMoCuNb 25-20 1.4500NiCrMoCu- and X5 NiCrMoCuTi 20-18 1.4506CrNiMoCu-steel GX2 NiCrMoCuN 20-18 1.4531
GX2 NiCrMoCuN 25-20 1.4536X1 NiCrMoCu 25-20-5 1.4539
GX7 CrNiMoCuNb 18-18 1.4585X5 NiCrMoCuNb 22-18 1.4586
2.5 x 350 40 - 75 DC+ 43 72 0.96 19.9 79 1.593.2 x 350 60 - 105 DC+ 53 133 1.3 32.1 52 1.694.0 x 350 80 - 145 DC+ 61 220 1.8 48.0 32 1.56
* stub end = 35mm
1G 2F 2G 3G 4G 5Gup up
2.5 70 70 70 60 60 603.2 100 100 100 70 70 704.0 140 140 140 80
Application advicesDeviation: Chemical composition: - welding with heat input max. 1.5 kJ/mmSi = max. 1.0% AWS A5.4-92 = max. 0.75% - interpass temperature max. 150°C
GRINOX 65
![Page 34: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/34.jpg)
Diameter (mm)Length (mm)Unit:Pieces / unit (nominal)Net weight/unit (kg)
Classification
Welding positions Current type
Chemical composition (w%), typical, all weld metal and ferritenumber
Mechanical properties, all weld metal
General description
Packaging, available sizes and identification
Identification Imprint: Tip colour:
Liability: All information in this data sheet is based on the best available knowledge, is subject to changewithout notice and can only be considered as suitable for general guidance.
Fumes: Consult information on Welding Safety Sheet, available upon request
Condition Yield strength Tensile strength Elongation Impact ISO-V(J)(N/mm2) (N/mm2) (%)
As weldedRequired AWS A5.4-92
EN 1600-97Typical values
ISO/ASME
Approvals
94
AC / DC electr. +/-
TÜV UDT+ +
C Mn Si Cr Ni Mo N FN0.020 0.8 1.0 22.5 9.5 3.2 0.16 30-55
MDS GRINOX 62 3
2.5 3.2 4.0 5.0350 350 350 350
Box184 112 76 4.93.8 3.8 3.9 3.8
GRINOX 62 / 2209-16 red
GRINOX 62
EN 1600 : E 22 9 3 L N R 32
A rutile-basic electrode for duplex stainless steel weldingExcellent weldability for filling as well as for root runsApplicable up to a service temperature of 250°CHigh resistance to general corrosion, pitting and stress corrosion (PREN ~35)High yield strength > 500 N/mm2
Weldable on AC and DC
AWS A5.4-92 : E 2209-16*EN 1600-97 : E 22 9 3 NL R 32
* Deviations see remarks
PA/1G PB/2F PC/2G PF/3G up PE/4G PF/5G up142536
+20°C -30°C -40°C
not required min. 690 min. 20 not requiredmin. 450 min. 550 min. 20 not required
650 800 27 60 50 40
Temperature rangepressurized: -40 ...+250°Cscaling resistance: n.a.
![Page 35: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/35.jpg)
Sizes Current Current Arc time Energy Dep.rate Weight/ Electrodes/ kg Electrodes/Diam. x length range type 1000 pcs. kg weldmetal kg weldmetal
(mm) (A) (s)* E(kJ) H(kg/h) (kg) B 1/N
Welding positions:Diameter(mm) Current(A)
Remarks
Welding parameters, optimum fill passes
Calculation data
Materials to be welded
- per electrode at max. current -
95
2.5 x 350 40 - 75 DC+ 61 127 0.73 20.6 81 1.673.2 x 350 80 - 110 DC+ 56 184 1.4 34.3 46 1.594.0 x 350 80 - 150 DC+ 59 205 2.0 51.5 30 1.525.0 x 350 140 - 220 DC+ 65 357 2.8 77.4 20 1.61
* stub end = 35mm
1G 2F 2G 3G 4G 5Gup up
2.5 70 70 70 60 60 603.2 100 100 100 70 70 704.0 140 140 140 805.0 180 180 180
For rootpasses DC- is recommended.
Deviation: Chemical composition: - welding with heat input max. 2.5 kJ/mmSi = max. 1.2%; - preheat and interpass temperature max. 150°CAWS A5.4-92 Si = max. 0.90%
GRINOX 62Steel grades EN 10088-1/-2 W.Nr. ASTM / ACI UNS
A240Duplex- X2 CrNiMoN 22 -5-3 1.4462 S31803stainless steel 1.4417 S31500
X3 CrNiMoN 27-5-2 1.4460 S31200X2 CrNiN 23-4 1.4362 S32304
Dissimilar joints such as un- and low alloyed steel to duplex stainless steel
Application advice
![Page 36: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/36.jpg)
Diameter (mm)Length (mm)Unit:Pieces / unit (nominal)Net weight/unit (kg)
Classification
Welding positions Current type
Chemical composition (w%), typical, all weld metal and ferritenumber
Mechanical properties, all weld metal
General description
Packaging, available sizes and identification
Identification Imprint: Tip colour:
Liability: All information in this data sheet is based on the best available knowledge, is subject to changewithout notice and can only be considered as suitable for general guidance.
Fumes: Consult information on Welding Safety Sheet, available upon request
Condition Yield strength Tensile strength Elongation Impact ISO-V(J)(N/mm2) (N/mm2) (%)
As weldedRequired AWS A5.4-92
EN 1600-97Typical values
ISO/ASME
Approvals
96
GRINOX 33
AWS A5.4-92: E 2209-15EN 1600-97 : E 22 9 3 NL B 22
DC electr. +
C Mn Si Cr Ni Mo N FN0.025 1.6 0.5 23.5 9.0 3.0 0.15 30-60
+20°C -20°C -40°C -50°C
not required min. 690 min. 20 not requiredmin. 450 min. 550 min. 20 not required
650 800 28 80 75 70 45
2.5 3.2 4.0250 350 350
Box116 783.8 3.8
GRINOX 33 /2209-15 red
MDS GRINOX 33 5
A basic all position electrode for duplex stainless steel weldingExcellent weldability for filling as well as for root runsApplicable up to a service temperature of 250°CHigh resistance to general corrosion, pitting and stress corrosion conditionsHigh yield strength > 500 N/mm2
Weldable on DC+ polarity
PA/1G PB/2F PC/2G PF/3G up PE/4G PF/5G up142536
0.2% Proof strength
Temperature rangepressurized: -40 ... +250°Cscaling resistance: n.a.
![Page 37: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/37.jpg)
Sizes Current Current Arc time Energy Dep.rate Weight/ Electrodes/ kg Electrodes/Diam. x length range type 1000 pcs. kg weldmetal kg weldmetal
(mm) (A) (s)* E(kJ) H(kg/h) (kg) B 1/N
Welding positions:Diameter(mm) Current(A)
Remarks
Welding parameters, optimum fill passes
Calculation data
Materials to be welded
- per electrode at max. current -
97
GRINOX 33
2.5 x 350 50 - 80 DC+ 74 101 0.62 21 78 1.643.2 x 350 70 - 110 DC+ 84 219 0.88 33.8 49 1.644.0 x 350 90 - 140 DC+
* stub end = 35mm
1G 2F 2G 3G 4G 5Gup up
AWS A5.4-92 : E 309L-16*EN 1600-97 : E 23 12 L R 32
* Deviations see remarks AC / DCelectr. +Approvals GL TÜV UDT
4332 + + C Mn Si Cr NiFN
0.020 0.8 1.0 23.0 12.5 10-20MDS GRINOX 733Steel Grades EN 10088-1/-2W.Nr.ASTM / ACI UNS
A240/A312/A351
Corrosion resisting X2 CrNiN 18-10 1.4311 (TP)304LN S30453
Cladsteel X2 CrNi 19-11 1.4306 (TP)304L S30403CF-3 J92500
X4 CrNi 18-10 1.4301 (TP)304 S30400
Steel grades EN 10088-1/-2 W.Nr. ASTM / ACI UNSA240
Duplex- X2 CrNiMoN 22 -5-3 1.4462 S31803stainless steel 1.4417 S31500
X3 CrNiMoN 27-5-2 1.4460 S31200X2 CrNiN 23-4 1.4362 S32304
Dissimilar joints such as un- and low alloyed steel to duplex stainless steel
- interpass temperature depending on construction
![Page 38: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/38.jpg)
Diameter (mm)Length (mm)Unit:Pieces / unit (nominal)Net weight/unit (kg)
Classification
Welding positions Current type
Chemical composition (w%), typical, all weld metal and ferritenumber
Mechanical properties, all weld metal
General description
Packaging, available sizes and identification
Identification Imprint: Tip colour:
Liability: All information in this data sheet is based on the best available knowledge, is subject to changewithout notice and can only be considered as suitable for general guidance.
Fumes: Consult information on Welding Safety Sheet, available upon request
Condition Yield strength Tensile strength Elongation Impact ISO-V(J)(N/mm2) (N/mm2) (%)
As weldedRequired AWS A5.4-92
EN 1600-97Typical values
ISO/ASME
Approvals
98
AWS A5.4-92 : E 309L-16*EN 1600-97 : E 23 12 L R 32
* Deviations see remarks
AC / DC electr. +
GL TÜV UDT4332 + +
C Mn Si Cr Ni FN0.020 0.8 1.0 23.0 12.5 10-20
MDS GRINOX 73 3
2.5 3.2 4.0 5.0350 350 450 450
Box152 110 68 453.2 3.8 4.9 4.9
GRINOX 73 / 309L-16 red
GRINOX 73
A rutile-basic all position CrNi over-alloyed buffer electrodeDeveloped for welding stainless steel to mild steel and for clad steelSelf releasing slagExcellent side wall wetting, no undercut, mirror like bead appearanceHigh resistance to porosityWeldable on AC and DC+ polarity
PA/1G PB/2F PC/2G PF/3G up PE/4G PF/5G up
+20°C -20°C
not required min. 520 min. 30 not requiredmin. 320 min. 510 min. 25 not required
480 560 40 55 50
142536
Temperature rangepressurized: -120 ...+350°Cscaling resistance: n.a.
0.2% Proof strength
![Page 39: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/39.jpg)
Sizes Current Current Arc time Energy Dep.rate Weight/ Electrodes/ kg Electrodes/Diam. x length range type 1000 pcs. kg weldmetal kg weldmetal
(mm) (A) (s)* E(kJ) H(kg/h) (kg) B 1/N
Welding positions:Diameter(mm) Current(A)
Remarks
Welding parameters, optimum fill passes
Calculation data
Materials to be welded
- per electrode at max. current -
99
Steel Grades EN 10088-1/-2 W.Nr. ASTM / ACI UNSA240/A312/A351
Corrosion resisting X2 CrNiN 18-10 1.4311 (TP)304LN S30453
Cladsteel X2 CrNi 19-11 1.4306 (TP)304L S30403CF-3 J92500
X4 CrNi 18-10 1.4301 (TP)304 S30400
- Dissimilar joints (mild and low alloyed steel to CrNi or CrNiMo stainless steel)- Build-up welding on mild and low alloyed steel- Butterlayer CrNi-cladsteel
2.5 x 350 45 - 80 DC+ 48 95 0.99 22.1 77 1.693.2 x 350 80 - 115 DC+ 56 160 1.4 35.1 46 1.594.0 x 450 100 - 155 DC+ 76 317 2.0 69.9 23 1.645.0 x 450 150 - 220 DC+ 84 575 2.9 108.0 15 1.59
* stub end = 35mm
Deviation: Chemical composition:Si max. 1.2%AWS A5.4-92: max. 0.90%
1G 2F 2G 3G 4G 5Gup up
2.5 70 70 70 60 60 603.2 100 100 100 70 70 704.0 140 140 1405.0 180 180
GRINOX 73
![Page 40: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/40.jpg)
Diameter (mm)Length (mm)Unit:Pieces / unit (nominal)Net weight/unit (kg)
Classification
Welding positions Current type
Chemical composition (w%), typical, all weld metal and ferritenumber
Mechanical properties, all weld metal
General description
Packaging, available sizes and identification
Identification Imprint: Tip colour:
Liability: All information in this data sheet is based on the best available knowledge, is subject to changewithout notice and can only be considered as suitable for general guidance.
Fumes: Consult information on Welding Safety Sheet, available upon request
Condition Yield strength Tensile strength Elongation Impact ISO-V(J)(N/mm2) (N/mm2) (%)
As weldedRequired AWS A5.4-92
EN 1600-97Typical values
ISO/ASME
Approvals
100
AWS A5.4-92 : E309MoL-16EN 1600-97 : E 23 12 2 L R 32
AC / DC electr. +
GL TÜV UDT4439 + +
C Mn Si Cr Ni Mo FN0.02 0.8 0.8 23.0 12.5 2.7 15-25
MDS GRINOX 53 3
2.0 2.5 3.2 4.0 5.0300 350 350 350 450
Box209 153 102 68 442.8 3.7 4.0 3.8 4.8
GRINOX 53 / 309MoL-16 red
GRINOX 53
A high CrNiMo alloyed all position rutile-basic electrodeHigh corrosion resistanceSpecially developed for welding stainless steel to mild steel and root runs in claddingMax. plate thickness in butt welds ~ 12mmSuitable for repair welding in dissimilar joints and steels difficult to weldWeldable on AC and DC + polarity
PA/1G PB/2F PC/2G PF/3G up PE/4G PF/5G up142536
+20°C -20°C -60°C
not required min. 520 min. 30 not requiredmin. 350 min. 550 min. 25 not required
580 700 30 57 50 45
Temperature rangepressurized: -10 ... +400°Cscaling resistance: n.a.
0.2% Proof strength
![Page 41: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/41.jpg)
Sizes Current Current Arc time Energy Dep.rate Weight/ Electrodes/ kg Electrodes/Diam. x length range type 1000 pcs. kg weldmetal kg weldmetal
(mm) (A) (s)* E(kJ) H(kg/h) (kg) B 1/N
Welding positions:Diameter(mm) Current(A)
Remarks
Welding parameters, optimum fill passes
Calculation data
Materials to be welded
- per electrode at max. current -
101
2.0 x 300 30 - 60 DC+ 44 46 0.54 10.8 149 1.612.5 x 350 40 - 80 DC+ 52 90 0.91 20.4 76 1.543.2 x 350 60 - 80 DC+ 58 122 1.4 33.2 45 1.494.0 x 350 80 - 150 DC+ 64 259 1.9 51.6 30 1.545.0 x 450 140 - 190 DC+ 99 549 2.6 98.7 14 1.38
* stub end = 35mm
1G 2F 2G 3G 4G 5Gup up
2.0 45 45 40 40 402.5 70 70 70 60 60 603.2 100 100 100 70 70 704.0 140 140 140 805.0 180 180 180
GRINOX 53Steel grades EN 10088-1/-2 EN 102 13-4 W.Nr. ASTM/ACI UNS
A240/A312/A351First layer in X2 CrNiMo 17-12-2 1.4404 (TP)316L S31603CrNiMo- CF-3M J92800claddings X2 CrNiMo 18-14-3 1.4435 (TP)316L S31603
X2 CrNiMoN 17-11-2 1.4406 (TP)316LN S31653X2 CrNiMoN 17-13-3 1.4429X4 CrNiMo 17-12-2 1.4401 (TP)316 S31600X4 CrNiMo 17-13-3 1.4436X6 CrNiMoTi 17-12-2 1.4571 316Ti S31635X10 CrNiMoTi 17-3 1.4573 316Ti S31635X6 CrNiMoNb 17-12-2 1.4580 316Cb
S31640GX5 CrNiMo 19-11 1.4408
- Welding dissimilar metals: mild steel or low alloyed steel to stainless CrNiMo-steel up to max. thickness of12mm.- Build-up welding on mild or low alloyed steel
![Page 42: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/42.jpg)
Diameter (mm)Length (mm)Unit:Pieces / unit (nominal)Net weight/unit (kg)
Classification
Welding positions Current type
Chemical composition (w%), typical, all weld metal and ferritenumber
Mechanical properties, all weld metal
General description
Packaging, available sizes and identification
Identification Imprint: Tip colour:
Liability: All information in this data sheet is based on the best available knowledge, is subject to changewithout notice and can only be considered as suitable for general guidance.
Fumes: Consult information on Welding Safety Sheet, available upon request
Condition Yield strength Tensile strength Elongation Impact ISO-V(J)(N/mm2) (N/mm2) (%)
As weldedRequired AWS A5.4-92
EN 1600-97Typical values
ISO/ASME
Approvals
102
AWS A5.4-92 : E 308 MoL-16*EN 1600-97 : E 20 10 3 R 32
* Deviations see remarks
AC / DC electr. +
2.5 3.2 4.0 5.0350 350 350 350
Box194 112 803.9 3.9 4.0
GRINOX 54 / 308MoL-16 red
MDS GRINOX 54 3
TÜV UDT+ +
GRINOX 54
C Mn Si Cr Ni Mo FN0.025 0.8 1.0 20.0 9.5 2.3 >20
A rutile-basic all position electrode for welding dissimilar jointsThe general purpose electrode for repair weldingSuitable for hobby and professional applicationsExcellent bead appearence and slag releaseAlso applicable for joining steels difficult to weldWeldable on AC and DC+ polarity
Chemical composition (w%), typical, all weld metal and ferritenumber
PA/1G PB/2F PC/2G PF/3G up PE/4G PF/5G up142536
+20°C -20°C
not required min. 520 min. 35 not requiredmin. 400 min. 620 min. 20 not required
500 720 30 70 60
Temperature rangepressurized: -20 ... + 350°Cscaling resistance: n.a.
0.2% Proof strength
![Page 43: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/43.jpg)
Sizes Current Current Arc time Energy Dep.rate Weight/ Electrodes/ kg Electrodes/Diam. x length range type 1000 pcs. kg weldmetal kg weldmetal
(mm) (A) (s)* E(kJ) H(kg/h) (kg) B 1/N
Welding positions:Diameter(mm) Current(A)
Remarks
Welding parameters, optimum fill passes
Calculation data
Materials to be welded
- per electrode at max. current -
103
Deviation: chemical compositionSi = 0.4 - 1.2%: AWS A5.4-92: Si = max. 0.90%
GRINOX 54
2.5 x 300 40 - 75 DC+ 54 99 0.86 19.8 78 1.543.2 x 350 60 - 110 DC+ 52 132 1.5 35.6 46 1.544.0 x 350 80 - 150 DC+ 62 234 1.9 66.0 30 1.495.0 x 350 140 - 220 DC+ 66 365 2.8 104.7 19 1.52
* stub end = 35mm
1G 2F 2G 3G 4G 5Gup up
2.5 70 70 70 60 60 603.2 100 100 100 70 70 704.0 140 140 140 805.0 180 180 180
Steel grades EN 10088-1/-2 EN 102 13-4 W.Nr. ASTM/ACI UNSA240/A312/A351
First layer in X2 CrNiMo 17-12-2 1.4404 (TP)316L S31603CrNiMo- CF-3M J92800claddings X2 CrNiMo 18-14-3 1.4435 (TP)316L S31603
X2 CrNiMoN 17-11-2 1.4406 (TP)316LN S31653X2 CrNiMoN 17-13-3 1.4429X4 CrNiMo 17-12-2 1.4401 (TP)316 S31600X4 CrNiMo 17-13-3 1.4436X6 CrNiMoTi 17-12-2 1.4571 316Ti S31635X10 CrNiMoTi 17-3 1.4573 316Ti S31635X6 CrNiMoNb 17-12-2 1.4580 316Cb S31640
GX5 CrNiMo 19-11 1.4408
- Welding dissimilar metals: mild steel or low alloyed steel to stainless CrNi and CrNiMo-steel- Build-up welding on mild or low alloyed steel
![Page 44: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/44.jpg)
Diameter (mm)Length (mm)Unit:Pieces / unit (nominal)Net weight/unit (kg)
Classification
Welding positions Current type
Chemical composition (w%), typical, all weld metal and ferritenumber
Mechanical properties, all weld metal
General description
Packaging, available sizes and identification
Identification Imprint: Tip colour:
Liability: All information in this data sheet is based on the best available knowledge, is subject to changewithout notice and can only be considered as suitable for general guidance.
Fumes: Consult information on Welding Safety Sheet, available upon request
Condition Yield strength Tensile strength Elongation Impact ISO-V(J)(N/mm2) (N/mm2) (%)
As weldedRequired AWS A5.4-92
EN 1600-97Typical values
ISO/ASME
Approvals
104
AWS A5.4-92 : E 309Mo-26*EN 1600-97 : E 23 12 2 LR 53*
* Deviations see remarks
AC / DC electr. +
C Mn Si Cr Ni Mo FN0.05 0.7 1.0 23.7 12.8 2.4 >15
MDS GRINOX 153 4
3.2 4.0450 450
Box69 414.7 4.3
GRINOX 153/309Mo-26 red
GRINOX 153
GL UDT4431 +
A rutile-basic synthetic high recovery (160%) electrode for shipbuildingFor welding carbon steel to stainless steel in the down hand positionExcellent for fillet weldingHigh resistance to porosity on primed plate materialHigher welding current can be usedHigh deposit rateSmooth bead appearance and easy slag releaseWeldable on AC and DC+ polarity
PA/1G PB/2F
+ 20°C -20°C
not required min. 550 min. 30 not requiredmin. 350 min. 550 min. 25 not required
550 740 28 50 45
1 4
Temperature rangepressurized: -20...+350°Cscaling resistance: n.a.
![Page 45: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/45.jpg)
Sizes Current Current Arc time Energy Dep.rate Weight/ Electrodes/ kg Electrodes/Diam. x length range type 1000 pcs. kg weldmetal kg weldmetal
(mm) (A) (s)* E(kJ) H(kg/h) (kg) B 1/N
Welding positions:Diameter(mm) Current(A)
Remarks
Welding parameters, optimum fill passes
Calculation data
Materials to be welded
- per electrode at max. current -
105
3.2 x 450 140 - 170 DC+ 86 409 1.9 68.1 22 1.524.0 x 450 180 - 230 DC+ 80 644 3.0 105.5 15 1.59
* stub end = 35mm
1G 2F
3.2 175 1404.0 200 180
GRINOX 153Steel grades EN 10088-1/-2 EN 102 13-4 W.Nr. ASTM/ACI UNS
A240/A312/A351X2 CrNiMo 17-12-2 1.4404 (TP)316L S31603
CF-3M J92800X2 CrNiMo 18-14-3 1.4435 (TP)316L S31603X4 CrNiMo 17-12-2 1.4401 (TP)316 S31600X4 CrNiMo 17-13-3 1.4436X6 CrNiMoTi 17-12-2 1.4571 316Ti S31635X10 CrNiMoTi 17-3 1.4573 316Ti S31635X6 CrNiMoNb 17-12-2 1.4580 316Cb S31640
GX5 CrNiMo 19-11 1.4408
- Welding dissimilar metals: mild steel or low alloyed steel to stainless CrNi and CrNiMo-steel up to max. thickness of 12mm- Build-up welding on mild or low alloyed steel
Deviation: Chemical compositionSi: max. 1.0 AWS A5.4-92: max. 0.90%C: max. 0.05% EN 1600-97: max. 0.04%
![Page 46: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/46.jpg)
Diameter (mm)Length (mm)Unit:Pieces / unit (nominal)Net weight/unit (kg)
Classification
Welding positions Current type
Chemical composition (w%), typical, all weld metal and ferritenumber
Mechanical properties, all weld metal
General description
Packaging, available sizes and identification
Identification Imprint: Tip colour:
Liability: All information in this data sheet is based on the best available knowledge, is subject to changewithout notice and can only be considered as suitable for general guidance.
Fumes: Consult information on Welding Safety Sheet, available upon request
Condition Yield strength Tensile strength Elongation Impact ISO-V(J)(N/mm2) (N/mm2) (%)
As weldedRequired AWS A5.4-92
EN 1600-97Typical values
ISO/ASME
Approvals
106
C Mn Si Cr Ni0.08 0.7 1.2 25.0 4.5
EN 1600-97 : E 25 4 R 12*
* deviations see remarks
AC / DC electr. +
MDS GRITHERM 48 3
2.5 3.2 4.0350 350 350
Box155 122 813.9 3.9 4.1
GRITHERM 48 none
GRITHERM 48
A rutile-basic all position stainless steel electrodeTypical applications: - buffer electrode, hardfacing on mild steels
- welding Cr-steels- high corrosion resistance- high proof stress and tensile strength
A ferritic/austenitic structureGood weldability and easy slag releaseWeldable on AC and DC + polarity
Chemical composition (w%), typical, all weld metal and ferritenumber
PA/1G PB/2F PC/2G PF/3G up PE/4G PF/5G up142536
0.2% Proof strength
Temperature rangepressurized: -10 ... + 350°Cscaling resistance: +1100°C
+20°CAs weldedRequired: EN 1600-97 min. 400 min. 600 min. 15 not requiredTypical values 500 700 15 30
![Page 47: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/47.jpg)
Sizes Current Current Arc time Energy Dep.rate Weight/ Electrodes/ kg Electrodes/Diam. x length range type 1000 pcs. kg weldmetal kg weldmetal
(mm) (A) (s)* E(kJ) H(kg/h) (kg) B 1/N
Welding positions:Diameter(mm) Current(A)
Remarks
Welding parameters, optimum fill passes
Calculation data
Materials to be welded
- per electrode at max. current -
107
2.5 x 350 40 - 70 DC+ 59 94 0.73 19.5 85 1.643.2 x 350 60 - 110 DC+ 58 122 1.2 31.4 50 1.564.0 x 350 80 - 140 DC+ 72 273 1.5 46.5 34 1.59
* stub end = 35mm
1G 2F 2G 3G 4G 5Gup up
2.5 70 70 70 60 60 603.2 100 100 100 70 70 704.0 140 140 140 80
GRITHERM 48
Steel grades EN 10088-1/-2 EN 102 13-4 W.Nr. ASTM/ACIBase metals GX30 CrSi 6 1.4710for high X10 CrSi 6 1.4712 502temperature X10 CrAl 7 1.4713 502application 403/405-TP405-CA15Center of weld X10 CrAl 13 1.4724 410/414-TP405-CA15to be weld GX40 CrSi 17 1.4740with Arosta 309S X10 CrAl 18 1.4742 430B-TP430-CB30cap layers GX40 CrSi 23 1.4745 TP433welded with X10 CrAl 24 1.4762 TP443Arosta 329 X20 CrNiSi 25-4 1.4821 TP329
GX40 CrNi 24-5 1.4822 TP329GX40 CrNiSi 27-4 1.4823 TP329HC
- Applications at high temperature when high Ni-content is unacceptable- Also very well suitable for hard surfacing in sea water corrosion resisting application
Deviation: chemical compositionSi = max. 1.5%; EN 1600-97 Si = max. 1.2%
![Page 48: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/48.jpg)
Diameter (mm)Length (mm)Unit:Pieces / unit (nominal)Net weight/unit (kg)
Classification
Welding positions Current type
Chemical composition (w%), typical, all weld metal and ferritenumber
Mechanical properties, all weld metal
General description
Packaging, available sizes and identification
Identification Imprint: Tip colour:
Liability: All information in this data sheet is based on the best available knowledge, is subject to changewithout notice and can only be considered as suitable for general guidance.
Fumes: Consult information on Welding Safety Sheet, available upon request
Condition Yield strength Tensile strength Elongation Impact ISO-V(J)(N/mm2) (N/mm2) (%)
As weldedRequired AWS A5.4-92
EN 1600-97Typical values
ISO/ASME
Approvals
108
GRINOX 29 red
AWS A5.4-92 : E 312-16*EN 1600-97 : E 29 9 R 12
* Deviations see remarks
AC / DC electr. +
MDS GRINOX 29 3
1.5 2.0 2.5 2.5 3.2 4.0 5.0250 300 250 350 350 350 350
Box470 263 174 176 122 82 562.6 3.4 2.6 3.7 4.0 4.0 4.0
GRINOX 29
DB UDT+ +
A rutile-basic high CrNi-alloyed all position electrodeExcellent for repair weldingSpecially developed for welding steels difficult to weld such as:- armour plate - austenitic Mn-steel - high C-steelExcellent weldability and self releasing slagWeldable on AC and DC+ polarity
C Mn Si Cr Ni0.11 0.9 1.0 29.0 9.0
+20°C
not required min. 660 min. 22 not requiredmin. 450 min. 650 min. 15 not required
700 800 20 50
PA/1G PB/2F PC/2G PF/3G up PE/4G PF/5G up142536
0.2% Proof strength
Temperature rangepressurized: -10 ... +350°Cscaling resistance: n.a.
![Page 49: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/49.jpg)
Sizes Current Current Arc time Energy Dep.rate Weight/ Electrodes/ kg Electrodes/Diam. x length range type 1000 pcs. kg weldmetal kg weldmetal
(mm) (A) (s)* E(kJ) H(kg/h) (kg) B 1/N
Welding positions:Diameter(mm) Current(A)
Remarks
Welding parameters, optimum fill passes
Calculation data
Materials to be welded
- per electrode at max. current -
109
1G 2F 2G 3G 4G 5Gup up
1.52.02.5 70 70 70 60 60 603.2 100 90 100 65 65 654.0 130 125 130 805.0
Deviation: Chemical composition:Si max. 1.2%AWS A5.4-92: max. 0.90%
Various steels grades as:
- Armour plate- Hardenable steels including steels difficult to weld- Non-magnetic austenitic steels- Work hardening austenitic manganese steels- Dissimilar steel grades (CMn-steels to stainless steel) up to max. thickness of 12 mm
1.5 x 250 30 - 402.0 x 300 40 - 55 DC+ 41 45 0.59 12.0 150 1.802.5 x 250 50 - 702.5 x 350 50 - 70 DC+ 57 91 0.73 20.7 87 1.793.2 x 350 70 - 100 DC+ 60 126 1.1 33.0 52 1.724.0 x 350 100 - 130 DC+ 72 273 1.4 49.7 35 1.725.0 x 350 130 - 140 DC+ 79 313 2.4 71.5 19 1.36
* stub end = 35mm
GRINOX 29
![Page 50: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/50.jpg)
Diameter (mm)Length (mm)Unit:Pieces / unit (nominal)Net weight/unit (kg)
Classification
Welding positions Current type
Chemical composition (w%), typical, all weld metal and ferritenumber
Mechanical properties, all weld metal
General description
Packaging, available sizes and identification
Identification Imprint: Tip colour:
Liability: All information in this data sheet is based on the best available knowledge, is subject to changewithout notice and can only be considered as suitable for general guidance.
Fumes: Consult information on Welding Safety Sheet, available upon request
Condition Yield strength Tensile strength Elongation Impact ISO-V(J)(N/mm2) (N/mm2) (%)
As weldedRequired AWS A5.4-92
EN 1600-97Typical values
ISO/ASME
Approvals
110
AWS A5.4-92 : E 312-16*EN 1600-97 : E 29 9 R 32*
* Deviations see remarks
AC/DC electr. +
2.0 2.5 3.2 4.0300 250 350 350
Box194 104 682.7 3.6 3.6
MDS GRINOX 592 3
GRINOX 592
C Mn Si Cr Ni0.11 0.9 1.2 29.5 9.0
GRINOX 592 / 312-16 red
A rutile-basic high CrNi-alloyed all position electrodeExcellent for repair weldingSpecially developed for welding steels difficult to weld such as:- armour plate - austenitic Mn-steel - high C-steelExcellent weldability and self releasing slagWeldable on AC and DC+ polarity Temperature range
pressurized: -10 ... +350°Cscaling resistance: n.a.
Chemical composition (w%), typical, all weld metal and ferritenumber
PA/1G PB/2F PC/2G PF/3G up PE/4G14253
0.2% Proof strength-20°C
RequiredAs welded AWS A5.4-92 not required min. 660 min. 22 not required EN 1600-97 min. 450 min. 650 min. 15 not requiredTypical values 700 800 20 50
![Page 51: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/51.jpg)
Sizes Current Current Arc time Energy Dep.rate Weight/ Electrodes/ kg Electrodes/Diam. x length range type 1000 pcs. kg weldmetal kg weldmetal
(mm) (A) (s)* E(kJ) H(kg/h) (kg) B 1/N
Welding positions:Diameter(mm) Current(A)
Remarks
Welding parameters, optimum fill passes
Calculation data
Materials to be welded
- per electrode at max. current -
111
Deviation: Chemical composition:Si max. 1.4%AWS A5.4-92: Si max. 0.90%; EN 1600-97: Si = max. 1.2%
GRINOX 592
Various steels grades as:
- Armour plate- Hardenable steels including steels difficult to weld- Non-magnetic austenitic steels- Work hardening austenitic manganese steels- Dissimilar steel grades (CMn-steels to stainless steel)
2.0 x 300 40 - 55 DC+ 41 45 0.59 12.0 150 1.802.5 x 350 50 - 70 DC+ 57 91 0.73 20.7 87 1.793.2 x 350 70 - 100 DC+ 60 126 1.1 33.0 52 1.724.0 x 350 100 - 130 DC+ 72 273 1.4 49.7 35 1.72
* stub end = 35mm
1G 2F 2G 3G 4G 5Gup up
2.02.5 70 70 70 60 60 603.2 100 90 100 65 65 654.0 130 125 130 80
![Page 52: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/52.jpg)
Diameter (mm)Length (mm)Unit:Pieces / unit (nominal)Net weight/unit (kg)
Classification
Welding positions Current type
Chemical composition (w%), typical, all weld metal and ferritenumber
Mechanical properties, all weld metal
General description
Packaging, available sizes and identification
Identification Imprint: Tip colour:
Liability: All information in this data sheet is based on the best available knowledge, is subject to changewithout notice and can only be considered as suitable for general guidance.
Fumes: Consult information on Welding Safety Sheet, available upon request
Condition Yield strength Tensile strength Elongation Impact ISO-V(J)(N/mm2) (N/mm2) (%)
As weldedRequired AWS A5.4-92
EN 1600-97Typical values
ISO/ASME
Approvals
112
AC/DC electr. +
2.5 3.2 4.0350 350 350
Box185 115 804.0 4.0 4.1
GRINOX 26 / 307-16 dark blue
MDS GRINOX 26 3
AWS A5.4-92 : E 307-16*EN 1600-97 : E 18 8 Mn R 12
* Deviations see remarks
ApprovalsDB TÜV UDT+ + +
GRINOX 26
A rutile- basic all position 5%Mn-alloyed stainless steel electrodeEspecially developed for steels difficult to weld, such as:- armour plate- austenitic high Mn-steelsOften used for buffer layers in "hardfacing" applicationsWeldable on AC and DC+ polarity Temperature range
pressurized: -60 ...+350°Cscaling resistance: n.a.
Chemical composition (w%), typical, all weld metal and ferritenumberC Mn Si Cr Ni
0.09 5.0 0.6 18.5 8.5
PA/1G PB/2F PC/2G PF/3G up PE/4G PF/5G up142536
0.2% Proof strength+20°C -60°C
As weldedRequired: AWS A5.4-92 not required min. 590 min. 30 not required EN 1600-97 min. 350 min. 500 min. 25 not requiredTypical values 450 650 35 110 75
![Page 53: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/53.jpg)
Sizes Current Current Arc time Energy Dep.rate Weight/ Electrodes/ kg Electrodes/Diam. x length range type 1000 pcs. kg weldmetal kg weldmetal
(mm) (A) (s)* E(kJ) H(kg/h) (kg) B 1/N
Welding positions:Diameter(mm) Current(A)
Remarks
Welding parameters, optimum fill passes
Calculation data
Materials to be welded
- per electrode at max. current -
113
Various steel grades as: Armour plateHardenable steels including steels difficult to weldNon-magnetic austenitic steelsWork hardening austenitic manganese steelsDissimilar steel grades (CMn-steels to stainless steel)Problem steels
2.5 x 350 70 - 80 DC+ 52 108 0.74 20.4 94 1.923.2 x 350 90 - 120 DC+ 56 148 1.2 34.7 54 1.874.0 x 350 110 - 140 DC+ 84 251 1.3 53.6 33 1.77
* stub end = 35mm
1G 2F 2G 3G 4G 5Gup up
2.5 80 80 80 80 80 803.2 100 100 100 904.0 140 115 130 110
Deviation: Chemical compositionMn = 4.5 - 6.0%;AWS A5.4-92: 3.30 - 4.75%
GRINOX 26
![Page 54: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/54.jpg)
Diameter (mm)Length (mm)Unit:Pieces / unit (nominal)Net weight/unit (kg)
Classification
Welding positions Current type
Chemical composition (w%), typical, all weld metal and ferritenumber
Mechanical properties, all weld metal
General description
Packaging, available sizes and identification
Identification Imprint: Tip colour:
Liability: All information in this data sheet is based on the best available knowledge, is subject to changewithout notice and can only be considered as suitable for general guidance.
Fumes: Consult information on Welding Safety Sheet, available upon request
Condition Yield strength Tensile strength Elongation Impact ISO-V(J)(N/mm2) (N/mm2) (%)
As weldedRequired AWS A5.4-92
EN 1600-97Typical values
ISO/ASME
Approvals
114
AWS A5.4-92 : E307-15*EN 1600-97 : E18 8 Mn B 22
* Deviations see remarks
AC/DC electr. +
2.5 3.2 4.0 6.0350 350 450 450
Box198 123 83 403.7 3.9 5.0 5.3
GRINOX 25 / 307-15 red
MDS GRINOX 25 3
ApprovalsDB TÜV UDT+ + +
GRINOX 25
A fully basic all position 5%Mn-alloyed stainless steel electrodeEspecially developed for steels difficult to weld, such as:- armour plate- austenitic high Mn-steelsOften used for buffer layers in "hardfacing" applicationsWeldable on DC+ polarity Temperature range
pressurized: -120 ... + 400°Cscaling resistance: n.a.
Chemical composition (w%), typical, all weld metal and ferritenumberC Mn Si Cr Ni
0.08 5.5 0.3 19.0 8.5
PA/1G PB/2F PC/2G PF/3G up PE/4G PF/5G up142536
0.2% Proof strength+20°C -120°C
As weldedRequired: AWS A5.4-92 not required min. 590 min. 30 not required EN 1600-97 min. 350 min. 500 min. 25 not requiredTypical values 500 700 35 140 35
![Page 55: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/55.jpg)
Sizes Current Current Arc time Energy Dep.rate Weight/ Electrodes/ kg Electrodes/Diam. x length range type 1000 pcs. kg weldmetal kg weldmetal
(mm) (A) (s)* E(kJ) H(kg/h) (kg) B 1/N
Welding positions:Diameter(mm) Current(A)
Remarks
Welding parameters, optimum fill passes
Calculation data
Materials to be welded
- per electrode at max. current -
115
Various steel grades as: Armour plateHardenable steels including steels difficult to weldNon-magnetic austenitic steelsWork hardening austenitic manganese steelsDissimilar steel grades (CMn-steels to stainless steel)Problem steel
2.5 x 350 50 - 70 DC+ 44 71 0.96 17.8 85 1.523.2 x 350 70 - 100 DC+ 53 132 1.4 29.1 48 1.394.0 x 450 100 - 130 DC+ 86 264 1.7 55.9 25 1.416.0 x 450 170 - 200 DC+
* stub end = 35mm
1G 2F 2G 3G 4G 5Gup up
2.5 60 60 60 60 60 603.2 90 90 90 704.0 140 115 130 956.0
Deviation: Chemical compositionMn = 4.5 - 6.5%; Ni = 7.5 - 9.5%AWS A5.4-92: Mn 3.30 - 4.75%; AWS A5.4-92: Ni = 9.0 - 10.7%
GRINOX 25
![Page 56: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/56.jpg)
Diameter (mm)Length (mm)Unit:Pieces / unit (nominal)Net weight/unit (kg)
Classification
Welding positions Current type
Chemical composition (w%), typical, all weld metal and ferritenumber
Mechanical properties, all weld metal
General description
Packaging, available sizes and identification
Identification Imprint: Tip colour:
Liability: All information in this data sheet is based on the best available knowledge, is subject to changewithout notice and can only be considered as suitable for general guidance.
Fumes: Consult information on Welding Safety Sheet, available upon request
Condition Yield strength Tensile strength Elongation Impact ISO-V(J)(N/mm2) (N/mm2) (%)
As weldedRequired AWS A5.4-92
EN 1600-97Typical values
ISO/ASME
Approvals
116
AWS A5.4-92 : E 307-26*EN 1600-97 : E 18 8 Mn R 53
* Nearest classification, see remarks
AC/DC electr. +
2.5 3.2 4.0 5.0250 350 450 450
Box116 76 49 302.5 3.8 4.8 4.6
GRINOX 126 / 307-26 red
MDS GRINOX 126 3
Approvals
GRINOX 126
C Mn Si Cr Ni0.06 5.0 0.6 18.0 8.0
A rutile 6%Mn-alloyed stainless steel electrodeEspecially developed for steels difficult to weld, such as:- armour plate- austenitic high Mn-steelsOften used for buffer layers in "hardfacing" applicationsWeldable on DC+ polarity
DB TÜV UDT+ + +
PA/1G PB/2F
Chemical composition (w%), typical, all weld metal and ferritenumber
1 4
+20°CAs weldedRequired: AWS A5.4-92 not required min. 590 min. 30 not required EN 1600-97 min. 350 min. 500 min. 25 not requiredTypical values 425 650 35 85
![Page 57: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/57.jpg)
Sizes Current Current Arc time Energy Dep.rate Weight/ Electrodes/ kg Electrodes/Diam. x length range type 1000 pcs. kg weldmetal kg weldmetal
(mm) (A) (s)* E(kJ) H(kg/h) (kg) B 1/N
Welding positions:Diameter(mm) Current(A)
Remarks
Welding parameters, optimum fill passes
Calculation data
Materials to be welded
- per electrode at max. current -
117
Deviation: Chemical compositionMn = 4.5 - 7.5%; Cr = 18.0 - 21.5%, Ni = 7.0 - 10.0%AWS A5.4-92: Mn 3.30 - 4.75%; AWS A5.4-92: Cr 18.0 - 21.5%; AWS A5.4-92: Ni 9.0-10.7%
GRINOX 126
Various steel grades as: Armour plateHardenable steels including steels difficult to weldNon-magnetic austenitic steelsWork hardening austenitic manganese steelsDissimilar steel grades (CMn-steels to stainless steel)
2.5 x 250 80 - 100 DC+ 44 71 0.96 17.8 85 1.523.2 x 350 110 - 150 DC+ 53 132 1.4 29.1 48 1.394.0 x 450 140 - 200 DC+ 86 264 1.7 55.9 25 1.415.0 x 450 210 - 260 DC+ 82 388 2.7 85.3 16 1.39
* stub end = 35 mm
1G 2F 2G
2.5 60 60 603.2 90 90 904.0 140 115 1305.0 160 165
![Page 58: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/58.jpg)
Diameter (mm)Length (mm)Unit:Pieces / unit (nominal)Net weight/unit (kg)
Classification
Welding positions Current type
Chemical composition (w%), typical, all weld metal and ferritenumber
Mechanical properties, all weld metal
General description
Packaging, available sizes and identification
Identification Imprint: Tip colour:
Liability: All information in this data sheet is based on the best available knowledge, is subject to changewithout notice and can only be considered as suitable for general guidance.
Fumes: Consult information on Welding Safety Sheet, available upon request
Condition Yield strength Tensile strength Elongation Impact ISO-V(J)(N/mm2) (N/mm2) (%)
As weldedRequired AWS A5.4-92
EN 1600-97Typical values
ISO/ASME
Approvals
118
AWS A5.4-92 : E309-16*EN 1600-97 : E 22 12 R 32*
* Deviations see remarks
AC / DC electr. +/-
C Mn Si Cr Ni FN0.10 0.8 1.6 22.0 11.0 3-8
MDS GRITHERM 44 3
2.5 3.2 4.0350 350 350
Box182 116 773.9 4.0 4.0
GRITHERM 44 / 309-16 none
Approvals
GRITHERM 44
A rutile basic all position stainless steel electrodeSpecial developed for high temperature applications like industrial furnaces (ovens)High resistance to oxidation up to 1050°CWeldable on AC and DC
Temperature rangepressurized: -10 ...+400°Cscaling resistance: 1100°C
PA/1G PB/2F PC/2G PF/3G up PE/4G PF/5G up142536
+20°CAs weldedRequired: AWS A5.4-92 not required min. 550 min. 30 not required EN 1600-97 min. 350 min. 550 min. 25 not requiredTypical values 500 700 30 50
![Page 59: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/59.jpg)
Sizes Current Current Arc time Energy Dep.rate Weight/ Electrodes/ kg Electrodes/Diam. x length range type 1000 pcs. kg weldmetal kg weldmetal
(mm) (A) (s)* E(kJ) H(kg/h) (kg) B 1/N
Welding positions:Diameter(mm) Current(A)
Remarks
Welding parameters, optimum fill passes
Calculation data
Materials to be welded
- per electrode at max. current -
119
2.5 x 350 40 - 110 DC+ 47 71 1.1 19.7 73 1.443.2 x 350 60 - 110 DC+ 58 140 1.5 31.9 42 1.334.0 x 350 80 - 150 DC+ 58 226 2.2 53.7 29 1.55
* stub end = 35mm
1G 2F 2G 3G 4G 5Gup up
2.5 70 70 70 60 60 603.2 100 100 100 70 70 704.0 140 140 140 80
For rootpasses DC- is recommended.
Deviations: Chemical composition:Si max, 2.0%; AWS A5.4-92: max 0.90%; EN 1600-97: max. 1.2%Cr 21.0 - 23.0%; AWS A5.4-92: 22.0 - 25.0%;Ni 11.0 - 13.0%; AWS A5.4-92:12.0 - 14.0%
GRITHERM 44
Steel grades EN 10088-1/-2 EN 102 13-4 W.Nr. ASTM/ACIUNS
GX30CrSi6 1.4710X10 CrAl 7 1.4713 502X10 CrAl 13 1.4724 410/414-TP405-CA15
GX40 CrSi 13 1.4729GX40 CrSi 17 1.4740
X10 CrAl 18 1.4742 430-TP430-CB30X10 CrAl 24 1.4762 TP443
GX25 CrNiSi 18-9 1.4825J92502
GX40 CrNiSi 22-9 1.4826X15 CrNiSi 20-12 1.4828 TP309
S30900GX25 CrNiSi 20-14
X12 CrNiTi 18-9
![Page 60: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/60.jpg)
Diameter (mm)Length (mm)Unit:Pieces / unit (nominal)Net weight/unit (kg)
Classification
Welding positions Current type
Chemical composition (w%), typical, all weld metal and ferritenumber
Mechanical properties, all weld metal
General description
Packaging, available sizes and identification
Identification Imprint: Tip colour:
Liability: All information in this data sheet is based on the best available knowledge, is subject to changewithout notice and can only be considered as suitable for general guidance.
Fumes: Consult information on Welding Safety Sheet, available upon request
Condition Yield strength Tensile strength Elongation Impact ISO-V(J)(N/mm2) (N/mm2) (%)
As weldedRequired AWS A5.4-92
EN 1600-97Typical values
ISO/ASME
Approvals
120
GRITHERM 47
DC electr. +
AWS A-5.4-92 : E310-15*EN 1600-97 : E 25 20 B12
* Deviations see remarks
C Mn Si Cr Ni0.1 3.0 0.3 25.0 21.0
+20°C
not required min. 550 min. 30 not requiredmin. 350 min. 550 min. 20 not required
440 600 30 100
2.5 3.2 4.0350 350 350
Box232 161 1034.0 4.6 4.4
MDS GRITHERM 47 3
GRITHERM 47 / 310-15 none
Basic coated electrode for all position welding except vertical downFully austenitic weld metal with high Cr and Ni content for very high service temperatureHigh resistance against oxidation and scaling up to 1100°CAvoid service temperatures between 650 - 850°CWeldable on DC only
PA/1G PB/2F PC/2G PF/3G up PE/4G14253
0.2% Proof strength
pressurized :-20 ...+400°Cscaling resistance: 1100°C
Temperature range
![Page 61: mdsGritec-B3.p62-121](https://reader033.fdocuments.us/reader033/viewer/2022042503/552d61415503464a778b46fb/html5/thumbnails/61.jpg)
Sizes Current Current Arc time Energy Dep.rate Weight/ Electrodes/ kg Electrodes/Diam. x length range type 1000 pcs. kg weldmetal kg weldmetal
(mm) (A) (s)* E(kJ) H(kg/h) (kg) B 1/N
Welding positions:Diameter(mm) Current(A)
Remarks
Welding parameters, optimum fill passes
Calculation data
Materials to be welded
- per electrode at max. current -
121
GRITHERM 47
2.5 x 350 60 - 703.2 x 350 80 - 904.0 x 350 110 - 130
2.53.24.0
EN 10088-1/-2 EN 102 13-4 W.Nr. ASTM/ACI UNSA240/A351
Heat resisting X10 CrAl 24 1.4762steel GX25 CrNiSi 18-9 1.4825
GX40 CrNiSi 22-9 1.4826X15 CrNiSi 20-12 1.4828
GX25 CrNiSi 20-14 1.4832X15 CrNiSi 25-20 1.4841 310S S31008
CK20 J94202X12 CrNi 25-21 1.4845
GX40 CrNiSi 25-20 1.4848 HK40
Deviation: Chemical composition:Mn = max. 5.0%; AWS A5.4-92: Mn = max. 2.5%