Introduction to aerospace materials - Dandelon.com...6.8 Case study: casting defects causing engine...
Transcript of Introduction to aerospace materials - Dandelon.com...6.8 Case study: casting defects causing engine...
![Page 1: Introduction to aerospace materials - Dandelon.com...6.8 Case study: casting defects causing engine disc failure in United Airlines flight 232 151 7 Processing and machining of aerospace](https://reader033.fdocuments.us/reader033/viewer/2022041918/5e6ace19788c9b7e8616eeed/html5/thumbnails/1.jpg)
WOODHEAD PUBLISHING IN MATERIALS
Introductionto aerospacematerials
Adrian P. Mouritz
WPWOODHEADPUBLISHING
![Page 2: Introduction to aerospace materials - Dandelon.com...6.8 Case study: casting defects causing engine disc failure in United Airlines flight 232 151 7 Processing and machining of aerospace](https://reader033.fdocuments.us/reader033/viewer/2022041918/5e6ace19788c9b7e8616eeed/html5/thumbnails/2.jpg)
Introduction to aerospace nnaterials
fECHNISCHE UNIVERSITAT DARMSTADTFachgebiet Konstruktiver Leichtbau und BauweisenProf. Dr.-lng. Helmut Schumann64287 Darmstadt, PetersenstraBe 30
i a v > M ! C a. vim <J v i. •... u. > a <;;.
T2
TU DarmstadtFB Maschinenbau
60052
© Woodhead Publishing Limited, 2012
![Page 3: Introduction to aerospace materials - Dandelon.com...6.8 Case study: casting defects causing engine disc failure in United Airlines flight 232 151 7 Processing and machining of aerospace](https://reader033.fdocuments.us/reader033/viewer/2022041918/5e6ace19788c9b7e8616eeed/html5/thumbnails/3.jpg)
Related titles:
Welding and joining of aerospace materials(ISBN 978-1-84569-532-3)As the demands on aircraft and the materials from which they are manufactured increase,so do the demands on the techniques used to join them. Welding and joining of aerospacematerials reviews welding techniques such as inertia friction, laser and hybrid laser-arcwelding. It also discusses other joining techniques such as riveting, bonding and brazing.
Failure mechanisms in polymer matrix composites(ISBN 978-1-84569-750-1)Polymer matrix composites are replacing materials such as metals in industries such asaerospace, automotive and civil engineering. As composites are relatively new materials,more information on the potential risk of failure is needed to ensure safe design. This bookfocuses on three main types of failure: impact damage, delamination and fatigue. Chaptersin Parts I to IV describe the main types of failure mechanism and discuss testing methodsfor predicting failure in composites. Chapters in Parts V and VI discuss typical kinds of in-service failure and their implications for industry.
Aerodynamic measurements(ISBN 978-1-84569-992-5)Aerodynamic measurements presents a comprehensive review of the theoretical bases forexperimental techniques used in aerodynamics. Limitations of each method in terms ofaccuracy, response time and complexity are addressed. This book serves as a guide tochoosing the most pertinent technique for each type of flow field including: ID, 2D, 3D,steady or unsteady, subsonic, supersonic or hypersonic.
Details of these books and a complete list of titles from Woodhead Publishing can beobtained by:
• visiting our web site at www.woodheadpublishing.com• contacting Customer Services (e-mail: [email protected];
fax: +44 (0) 1223 832819; tel.: +44 (0) 1223 499140 ext. 130; address: WoodheadPublishing Limited, 80 High Street, Sawston, Cambridge CB22 3HJ, UK)
• in North America, contacting our US office (e-mail: [email protected]; tel.: (215) 928 9112; address: Woodhead Publishing, 1518 Walnut Street, Suite1100, Philadelphia, PA 19102-3406, USA)
If you would like e-versions of our content, please visit our online platform:www.woodheadpublishingonline.com. Please recommend it to your librarian so thateveryone in your institution can benefit from the wealth of content on the site.
© Woodhead Publishing Limited, 2012
![Page 4: Introduction to aerospace materials - Dandelon.com...6.8 Case study: casting defects causing engine disc failure in United Airlines flight 232 151 7 Processing and machining of aerospace](https://reader033.fdocuments.us/reader033/viewer/2022041918/5e6ace19788c9b7e8616eeed/html5/thumbnails/4.jpg)
introductionto aerospace
materials
Adrian P. Mouritz
rECHMiSCHE UMIVERSITAT DARMSTADTFachgebist Konstruktiver Leichtbau und BauweisenProf. Dr.-ing. Helmut Schlirmann^4287 Darmstadt, PetersenstraBe 30
WPWOODHEADPUBLISHING
iOxford Cambridge Philadelphia New Delhi
© Woodhead Publishing Limited, 2012
![Page 5: Introduction to aerospace materials - Dandelon.com...6.8 Case study: casting defects causing engine disc failure in United Airlines flight 232 151 7 Processing and machining of aerospace](https://reader033.fdocuments.us/reader033/viewer/2022041918/5e6ace19788c9b7e8616eeed/html5/thumbnails/5.jpg)
Published by Woodhead Publishing Limited,80 High Street, Sawston, Cambridge CB22 3HJ, UKwww.woodheadpublishing.comwww.woodheadpublishingonline.com
Woodhead Publishing, 1518 Walnut Street, Suite 1100, Philadelphia, PA 19102-3406, USA
Woodhead Publishing India Private Limited, G-2, Vardaan House, 7/28 Ansari Road,Daryaganj, New Delhi - 110002, Indiawww.woodheadpublishingindia.com
First published 2012, Woodhead Publishing Limited© Woodhead Publishing Limited, 2012The author has asserted his moral rights.
Every effort has been made to trace and acknowledge ownership of copyright. Thepublisher will be glad to hear from any copyright holders whom it has not been possible tocontact.
This book contains information obtained from authentic and highly regarded sources.Reprinted material is quoted with permission, and sources are indicated. Reasonable effortshave been made to publish reliable data and information, but the author and the publishercannot assume responsibility for the validity of all materials. Neither the author nor thepublisher, nor anyone else associated with this publication, shall be liable for any loss,damage or liability directly or indirectly caused or alleged to be caused by this book.
Neither this book nor any part may be reproduced or transmitted in any form or by anymeans, electronic or mechanical, including photocopying, microfilming and recording, or byany information storage or retrieval system, without permission in writing from WoodheadPublishing Limited.
The consent of Woodhead Publishing Limited does not extend to copying for generaldistribution, for promotion, for creating new works, or for resale. Specific permission mustbe obtained in writing from Woodhead Publishing Limited for such copying.
Trademark notice: Product or corporate names may be trademarks or registered trademarks,and are used only for identification and explanation, without intent to infringe.
British Library Cataloguing in Publication DataA catalogue record for this book is available from the British Library.
ISBN 978-1-85573-946-8 (print)ISBN 978-0-85709-515-2 (online)
The publisher's policy is to use permanent paper from mills that operate a sustainableforestry policy, and which has been manufactured from pulp which is processed using acid-free and elemental chlorine-free practices. Furthermore, the publisher ensures that the textpaper and cover board used have met acceptable environmental accreditation standards.
Typeset by Replika Press Pvt Ltd, IndiaPrinted by TJ International Ltd, Padstow, Cornwall, UK
Cover image © Christopher Weyer
pun nr
© Woodhead Publishing Limited, 2012
![Page 6: Introduction to aerospace materials - Dandelon.com...6.8 Case study: casting defects causing engine disc failure in United Airlines flight 232 151 7 Processing and machining of aerospace](https://reader033.fdocuments.us/reader033/viewer/2022041918/5e6ace19788c9b7e8616eeed/html5/thumbnails/6.jpg)
FECHNISCHE UNiVERSITAT DARMSTADTFachqebiet Konstruktiver Leichtbau und Bauweisen
Prof.'-Diving. Helmut Schurmann<U237 Darmstadt, petersenstra&e 30
Contents
Preface
Introduction to aerospace materials
Xlll
1.11.21.31.41.51.6
22.12:22.32.42.52.6
3
3.13.23.33.43.53.6
4
4.14.24.3
The importance of aerospace matenalsUnderstanding aerospace materialsIntroducing the main types of aerospace materialsWhat makes for a good aerospace material?SummaryFurther reading and research
Aerospace materials: past, present and futureIntroductionBrief history of aerospace materialsMaterials for the global aerospace industryFuture advances in aerospace materialsSummaryFurther reading and research
Materials and material requirements for aerospacestructures and enginesIntroductionFixed-wing aircraft structuresHelicopter structuresSpace shuttle structuresSummaryFurther reading and research
Strengthening of metal alloys
IntroductionCrystal structure of metalsDefects in crystal structures
124
111314
15
151932353738
39
394051545556
57
575860
© Woodhead Publishing Limited, 2012
![Page 7: Introduction to aerospace materials - Dandelon.com...6.8 Case study: casting defects causing engine disc failure in United Airlines flight 232 151 7 Processing and machining of aerospace](https://reader033.fdocuments.us/reader033/viewer/2022041918/5e6ace19788c9b7e8616eeed/html5/thumbnails/7.jpg)
VI Contents
4.4 Strengthening of metals 684.5 Summary 874.6 Terminology 884.7 Further reading and research 89
5 Mechanical and durability testing of aerospacematerials 91
5.1 Introduction 915.2 Tension test 925.3 Compression test 1065.4 Flexure test 1075.5 Hardness test 1085.6 Fracture test 1115.7 Drop-weight impact test 1135.8 Fatigue test 1145.9 Creep test 1155.10 Environmental durability testing 1165.11 Certification of aerospace materials 1185.12 Summary 1235.13 Terminology 1265.14 Further reading and research 127
6 Production and casting of aerospace metals 128
6.1 Introduction 1286.2 Production of metal alloys 1286.3 Casting of metal alloys 1346.4 Casting processes 1436.5 Summary 1496.6 Terminology 1506.7 Further reading and research 1516.8 Case study: casting defects causing engine disc failure in
United Airlines flight 232 151
7 Processing and machining of aerospace metals 154
7.1 Introduction 1547.2 Metal-forming processes 1567.3 Hot and cold working of metal products 1617.4 Powder metallurgy for production of aerospace
superalloys 1677.5 Machining of metals 1687.6 Summary 1707.7 Terminology 171
© Woodhead Publishing Limited, 2012
![Page 8: Introduction to aerospace materials - Dandelon.com...6.8 Case study: casting defects causing engine disc failure in United Airlines flight 232 151 7 Processing and machining of aerospace](https://reader033.fdocuments.us/reader033/viewer/2022041918/5e6ace19788c9b7e8616eeed/html5/thumbnails/8.jpg)
7.8
8
8.18.28.38.48.58.68.78.88.9
9
9.19.2
9.39.49.59.69.79.8
10
10.110.210.310.4
11
11.111.211.311.411.511.611.711.8
12
12.1
Contents
Further reading and research
Aluminium alloys for aircraft structures
IntroductionAluminium alloy typesNon-age-hardenable aluminium alloysAge-hardenable aluminium alloysSpeciality aluminium alloysHeat treatment of age-hardenable aluminium alloysHigh-temperature strength of aluminiumSummaryFurther reading and research
Titanium alloys for aerospace structures and engines
IntroductionTitanium alloys: advantages and disadvantages foraerospace applicationsTypes of titanium alloyTitanium aluminidesShape-memory titanium alloysSummaryTerminologyFurther reading and research
Magnesium alloys for aerospace structures
IntroductionMetallurgy of magnesium alloysSummaryFurther reading and research
Steels for aircraft structures
IntroductionBasic principles of steel metallurgyMaraging steelMedium-carbon low-alloy steelStainless steelSummaryTerminologyFurther reading and research
Superalloys for gas turbine engines
Introduction
vii
172
173
173175179181186188197200201
202
202
205207216218221222223
224
224225231231
232
232234244246246247249249
251
251
© Woodhead Publishing Limited, 2012
![Page 9: Introduction to aerospace materials - Dandelon.com...6.8 Case study: casting defects causing engine disc failure in United Airlines flight 232 151 7 Processing and machining of aerospace](https://reader033.fdocuments.us/reader033/viewer/2022041918/5e6ace19788c9b7e8616eeed/html5/thumbnails/9.jpg)
viii Contents
12.2 A simple guide to jet engine technology12.3 Nickel-based superalloys12.4 Iron-nickel superalloys12.5 Cobalt superalloys12.6 Thermal barrier coatings for jet engine alloys12.7 Advanced materials for jet engines12.8 Summary12.9 Further reading and research
13 Polymers for aerospace structures
13.1 Introduction13.2 Aerospace applications of polymers13.3 Advantages and disadvantages of polymers for
aerospace applications13.4 Polymerisation13.5 Thermosetting polymers13.6 Thermoplastics13.7 Elastomers13.8 Structural adhesives13.9 Mechanical properties of polymers13.10 Polymer additives13.11 Polymers for radar-absorbing materials (RAMs)13.12 Summary13.13 Terminology13.14 Further reading and research13.15 Case study: space shuttle Challenger accident
14 Manufacturing of fibre-polymer compositematerials
14.1 Introduction14.2 Fibre reinforcements for composites14.3 Production of prepregs and fabrics14.4 Core materials for sandwich composites14.5 Composites manufacturing using prepreg14.6 Composites manufacturing by resin infusion14.7 Machining of composites14.8 Summary14.9 Terminology14.10 Further reading and research14.11 Case study: carbon nanotubes in composites
254256262262263265265266
268
268270
270271276279283285288294296298299301301
303
303306315319321326333334335336336
© Woodhead Publishing Limited, 2012
![Page 10: Introduction to aerospace materials - Dandelon.com...6.8 Case study: casting defects causing engine disc failure in United Airlines flight 232 151 7 Processing and machining of aerospace](https://reader033.fdocuments.us/reader033/viewer/2022041918/5e6ace19788c9b7e8616eeed/html5/thumbnails/10.jpg)
Contents IX
15 Fibre-polymer composites for aerospacestructures and engines 338
15.1 Introduction 33815.2 Types of composite materials 33915.3 Aerospace applications of fibre-polymer composites 34215.4 Advantages and disadvantages of using fibre-polymer
composites 34815.5 Mechanics of continuous-fibre composites 35415.6 Sandwich composites 37815.7 Environmental durability of composites 38415.8 Summary 39015.9 Terminology 39215.10 Further reading and research 393
16 Metal matrix, fibre-metal and ceramic matrixcomposites for aerospace applications 394
16.1 Metal matrix composites 39416.2 Fibre-metal laminates 40016.3 Ceramic matrix composites 40216.4 Summary 40616.5 Terminology 40716.6 Further reading and research 40816.7 Case study: ceramic matrix composities in the space
shuttle orbiter 408
17 Wood in small aircraft construction 411
17.1 Introduction 41117.2 Advantages and disadvantages of wood 41217.3 Hardwoods and softwoods 41217.4 Structure and composition of wood 41417.5 Engineering properties of wood 41817.6 Summary 42417.7 Terminology 42517.8 Further reading and research 42617.9 Case study: Spruce Goose (Hughes H-4 Hercules) 426
18 Fracture processes of aerospace materials 428
18.1 Introduction 42818.2 Fracture processes of aerospace materials 43118.3 Stress concentration effects in materials 43918.4 Fracture mechanics 44418.5 Application of fracture mechanics to aerospace materials 448
© Woodhead Publishing Limited, 2012
![Page 11: Introduction to aerospace materials - Dandelon.com...6.8 Case study: casting defects causing engine disc failure in United Airlines flight 232 151 7 Processing and machining of aerospace](https://reader033.fdocuments.us/reader033/viewer/2022041918/5e6ace19788c9b7e8616eeed/html5/thumbnails/11.jpg)
x Contents
18.6 Summary 44918.7 Terminology 45018.8 Further reading and research 45118.9 Case study: fracture in the space shuttle Columbia disaster 45118.10 Case study: fracture of aircraft composite radome 452
19 Fracture toughness properties of aerospacematerials 454
19.119.219.319.419.519.619.7
20
20.120.220.320.420.520.620.720.820.920.1020.1120.12
21
21.121.221.321.421.521.621.721.8
22
22.1
IntroductionFracture toughness propertiesDuctile/brittle fracture transition for metalsImproving the fracture toughness of aerospace materialsSummaryTerminologyFurther reading and research
Fatigue of aerospace materialsIntroductionFatigue stressFatigue life (S-N) curvesFatigue-crack growth curvesFatigue of metalsFatigue of fibre-polymer compositesFretting, acoustic and thermal fatigueSummaryTerminologyFurther reading and researchCase study: aircraft fatigue in Japan Airlines flight 123Case study: metal fatigue in Comet aircraft accidents
Corrosion of aerospace metalsIntroductionCorrosion processTypes of corrosionCorrosion protection of metalsSummaryTerminologyFurther reading and researchCase study: corrosion in the Aloha Airlines flight 243
Creep of aerospace materialsIntroduction
454454463465467468468
469
469470475477480487492493494495495496
498
498501504513517517518519
521
521
© Woodhead Publishing Limited, 2012
![Page 12: Introduction to aerospace materials - Dandelon.com...6.8 Case study: casting defects causing engine disc failure in United Airlines flight 232 151 7 Processing and machining of aerospace](https://reader033.fdocuments.us/reader033/viewer/2022041918/5e6ace19788c9b7e8616eeed/html5/thumbnails/12.jpg)
Contents XI
22.2 Creep behaviour of materials22.3 Creep of metals22.4 Creep of polymers and polymer composites22.5 Creep-resistant materials22.6 Summary22.7 Terminology22.8 Further reading and research
23 Nondestructive inspection and structural healthmonitoring of aerospace materials
23.1 Introduction23.2 Nondestructive inspection methods23.3 Structural health monitoring (SHM)23.4 Summary23.5 Terminology23.6 Further reading and research
24 Disposal and recycling of aerospace materials
24.1 Introduction24.2 Metal recycling24.3 Composite recycling24.4 Summary24.5 Further reading and research
25 Materials selection for aerospace
25.1 Introduction25.2 Materials selection in design25.3 Stages of materials selection25.4 Materials property charts25.5 Structural properties in materials selection25.6 Economic and business considerations in materials
selection25.7 Manufacturing considerations in materials selection25.8 Durability considerations in materials selection25.9 Environmental considerations in materials selection25.10 Specialist properties in materials selection25.11 Summary25.12 Terminology25.13 Further reading and research
Index
522525526530532533533
534
534537548553555557
558
558562566568568
569
569571574580582
586589593597597598599600
607