Handbook and damage atlas for inspection of glass fiber ... · Handbook and damage atlas for...

32
Handbook and damage atlas for inspection of glass fiber reinforced plastics Polymeric researcher, Swerea KIMAB [email protected] Klas Esbo 1

Transcript of Handbook and damage atlas for inspection of glass fiber ... · Handbook and damage atlas for...

Page 1: Handbook and damage atlas for inspection of glass fiber ... · Handbook and damage atlas for inspection of glass fiber reinforced plastics Polymeric researcher, Swerea KIMAB Klas.esbo@swerea.se

Handbook and damage atlas for

inspection of glass fiber reinforced

plastics

Polymeric researcher, Swerea KIMAB

[email protected]

Klas Esbo

1

Page 2: Handbook and damage atlas for inspection of glass fiber ... · Handbook and damage atlas for inspection of glass fiber reinforced plastics Polymeric researcher, Swerea KIMAB Klas.esbo@swerea.se

KIMAB Swerea KIMAB is one of the oldest Swedish research institute- founded

1921 and it is a merge between the corrosion institute and the institute for

metal research

Gunnar Bergman started year 1981 the polymer group

Page 3: Handbook and damage atlas for inspection of glass fiber ... · Handbook and damage atlas for inspection of glass fiber reinforced plastics Polymeric researcher, Swerea KIMAB Klas.esbo@swerea.se

Polymeric Materials

Chemical industry

Paper and Pulp

Plastic Joining Nuclear power

Steel industry

Pickling

Water and

waste water

Chlor/Alkali

Desinfection

Relining

Flue gas

cleaning

Page 4: Handbook and damage atlas for inspection of glass fiber ... · Handbook and damage atlas for inspection of glass fiber reinforced plastics Polymeric researcher, Swerea KIMAB Klas.esbo@swerea.se

4

Karin

Jacobson

Group Leader

Polymeric Materials

Daniel

Ejdeholm

Research Leader

e

Martina Källrot

Janstål

Researcher

Love

Pallonen

Researcher

Dinko

Lukes

Researcher

4

Nina Pendergraph

Researcher

Kenny Constanzo

Researcher

Klas Esbo

Researcher

Page 5: Handbook and damage atlas for inspection of glass fiber ... · Handbook and damage atlas for inspection of glass fiber reinforced plastics Polymeric researcher, Swerea KIMAB Klas.esbo@swerea.se

Agenda

• Introduction

-Thermosetting resin

-Glass fiber

• Failures and damages

-Common failures

• Inspection

-Destructive

-Non destructive

• Conclusion

5

Page 6: Handbook and damage atlas for inspection of glass fiber ... · Handbook and damage atlas for inspection of glass fiber reinforced plastics Polymeric researcher, Swerea KIMAB Klas.esbo@swerea.se

Introduction

6

Polymer

Glass fibers

Glass fiber reinforced

plastic (FRP)

Page 7: Handbook and damage atlas for inspection of glass fiber ... · Handbook and damage atlas for inspection of glass fiber reinforced plastics Polymeric researcher, Swerea KIMAB Klas.esbo@swerea.se

Introduction

7

Thermosetting Resin

Glass fibers

Glass fiber reinforced

plastic (FRP or GRP)

Different types

Polymer

Initiator

Different structures

Page 8: Handbook and damage atlas for inspection of glass fiber ... · Handbook and damage atlas for inspection of glass fiber reinforced plastics Polymeric researcher, Swerea KIMAB Klas.esbo@swerea.se

Different termosetting resin

8

Thermosetting Resin

Vinyl ester

Bisphenol-A

fumarate

Terephthalic

polyester

Isophthalic

polyester Chlorendic

polyester

Page 9: Handbook and damage atlas for inspection of glass fiber ... · Handbook and damage atlas for inspection of glass fiber reinforced plastics Polymeric researcher, Swerea KIMAB Klas.esbo@swerea.se

Different initiator for thermosetting resins

9

Thermosetting Resin

Methyl Ethyl

Ketone Peroxide

(MEKP)

Cumene

Hydroperoxide

(CHP)

Benzoyl

Peroxide (BPO)

Page 10: Handbook and damage atlas for inspection of glass fiber ... · Handbook and damage atlas for inspection of glass fiber reinforced plastics Polymeric researcher, Swerea KIMAB Klas.esbo@swerea.se

Different additives for thermosetting resins

10

Thermosetting Resin

Inhibitors

Accelerators

Fillers and

Pigments

Other additives

Page 11: Handbook and damage atlas for inspection of glass fiber ... · Handbook and damage atlas for inspection of glass fiber reinforced plastics Polymeric researcher, Swerea KIMAB Klas.esbo@swerea.se

Different glass fibers and structures

11

Glass fiber

structure

Chopped strand

mat (CSM)

Woven Roving

3D-woven

Surface veil

Roving

Glass fiber

E-

Glass

C-Glass

ECR-Glass

A-Glass

Page 12: Handbook and damage atlas for inspection of glass fiber ... · Handbook and damage atlas for inspection of glass fiber reinforced plastics Polymeric researcher, Swerea KIMAB Klas.esbo@swerea.se

Structural laminate, designed according to actual mechanical stresses.

Corrosion barrier, normally 2.5 mm thick. Protects the structural laminate from chemical attack.

Hand laid-up laminate

Structural laminate, alternating layers of woven roving (WR) and mats of chopped strand mat (CSM)

Corrosion barrier

Fibre-wound laminate Structural laminate, filament-wound with high fibre content

Corrosion barrier

Laminate build up for chemical environments

Page 13: Handbook and damage atlas for inspection of glass fiber ... · Handbook and damage atlas for inspection of glass fiber reinforced plastics Polymeric researcher, Swerea KIMAB Klas.esbo@swerea.se

Regulations and standards

13

• Regulations and standards verify that the level of quality inherent in the

specifications is, in fact, delivered to the purchaser

• Important regulations for Sweden are pressure equipment directive

(PED), AFS 2016:1 (AFS Arbetsmiljöverkets författningssamling) and

MSBs (Myndigheten för sammhällsskydd och beredskap) regulations

for tanks and pipelines

• Important standards for Sweden are EN 13121 (Behållare för kärl I

glasfiberaremerad plast för användning ovan jord), “PRN,

Plaströrsleningsnormer” and “PLN, plastkärlsnormer”

Page 14: Handbook and damage atlas for inspection of glass fiber ... · Handbook and damage atlas for inspection of glass fiber reinforced plastics Polymeric researcher, Swerea KIMAB Klas.esbo@swerea.se

Design of GRP/FRP

ASME Boiler and Pressure Vessel Code (BPVC)

Part B - Nonferrous Material Specifications

Supplementary part to other sections of the Code providing material

specifications for nonferrous materials

European norm EN 13121 parts 1-4

GRP tanks and vessels for use above ground

Part 1: Raw materials – Specification conditions and acceptance

conditions

Part 2: Chemical resistance

Part 3: Design and workmanship

Part 4: Delivery, installation and maintenance

Page 15: Handbook and damage atlas for inspection of glass fiber ... · Handbook and damage atlas for inspection of glass fiber reinforced plastics Polymeric researcher, Swerea KIMAB Klas.esbo@swerea.se

Failures

15

Page 16: Handbook and damage atlas for inspection of glass fiber ... · Handbook and damage atlas for inspection of glass fiber reinforced plastics Polymeric researcher, Swerea KIMAB Klas.esbo@swerea.se

Diffusion

• Polymers are permeable

• Diffusion of the media into the corrosion barrier is okay, but never

into the structural layer.

• Called weeping if it comes out through the FRP

• Microscope is the best inspection tool:

16

HCl diffusion Corrosion barrier

Structural layer

Page 17: Handbook and damage atlas for inspection of glass fiber ... · Handbook and damage atlas for inspection of glass fiber reinforced plastics Polymeric researcher, Swerea KIMAB Klas.esbo@swerea.se

Blisters

• Due to diffusions blisters are created by an osmotic process

• In general they are rather shallow and are situated close to the

surface under the corrosion barrier

17

Page 18: Handbook and damage atlas for inspection of glass fiber ... · Handbook and damage atlas for inspection of glass fiber reinforced plastics Polymeric researcher, Swerea KIMAB Klas.esbo@swerea.se

Delamination

• When different glass fiber sheets disconnect

• Could be due to heat changes

• In general more severe and lies deeper then blisters

• Can often be repaired or changed

18

Page 19: Handbook and damage atlas for inspection of glass fiber ... · Handbook and damage atlas for inspection of glass fiber reinforced plastics Polymeric researcher, Swerea KIMAB Klas.esbo@swerea.se

Discoloration

19

• Can be caused by many different reasons; temperature, chemicals,

Page 20: Handbook and damage atlas for inspection of glass fiber ... · Handbook and damage atlas for inspection of glass fiber reinforced plastics Polymeric researcher, Swerea KIMAB Klas.esbo@swerea.se

Impact damage

20

• Hard and sudden damage against the laminate

• In general rather shallow but could cause severe damage on the

inside

• Outside looks like round mark with scars

Inside looks like a star

Page 21: Handbook and damage atlas for inspection of glass fiber ... · Handbook and damage atlas for inspection of glass fiber reinforced plastics Polymeric researcher, Swerea KIMAB Klas.esbo@swerea.se

Stress corrosion cracking

• Tensile stresses together with certain chemicals cause stress

corrosion cracking

• The fibers reacts with the chemicals and can cause rapid raptures

• Extremely sensitive to impact damages

21

Page 22: Handbook and damage atlas for inspection of glass fiber ... · Handbook and damage atlas for inspection of glass fiber reinforced plastics Polymeric researcher, Swerea KIMAB Klas.esbo@swerea.se

All types of corrosion found in metals can also be found in plastics and rubber.

Uniform corrosion, wall thinning Stress corrosion Atmospheric corrosion, chalking Localized corrosion/pitting/crevice

corrosion Erosion corrosion Galvanic corrosion Filiform corrosion

Page 23: Handbook and damage atlas for inspection of glass fiber ... · Handbook and damage atlas for inspection of glass fiber reinforced plastics Polymeric researcher, Swerea KIMAB Klas.esbo@swerea.se

Cracks

23

• Surface cracks

• Drying cracks

• Structural cracks

Page 24: Handbook and damage atlas for inspection of glass fiber ... · Handbook and damage atlas for inspection of glass fiber reinforced plastics Polymeric researcher, Swerea KIMAB Klas.esbo@swerea.se

Inspections

24

Page 25: Handbook and damage atlas for inspection of glass fiber ... · Handbook and damage atlas for inspection of glass fiber reinforced plastics Polymeric researcher, Swerea KIMAB Klas.esbo@swerea.se

Destructive testing

25

Composition

Thermal history by

differential scanning

calometry (DSC)

Microscope

Chemical composition

by Fourier Transform

Infrared Spectroscopy

(FTIR)

Mechanical

strength

Page 26: Handbook and damage atlas for inspection of glass fiber ... · Handbook and damage atlas for inspection of glass fiber reinforced plastics Polymeric researcher, Swerea KIMAB Klas.esbo@swerea.se

Non-destructive testing

• Visual inspection

• Ultrasound

• X-ray

• Acoustic emission

• Barcol Hardness

26

Page 27: Handbook and damage atlas for inspection of glass fiber ... · Handbook and damage atlas for inspection of glass fiber reinforced plastics Polymeric researcher, Swerea KIMAB Klas.esbo@swerea.se

Calculations

• The vast variations of GAP and failures makes it difficult to make

calculations

• Weakest link?

27

Page 28: Handbook and damage atlas for inspection of glass fiber ... · Handbook and damage atlas for inspection of glass fiber reinforced plastics Polymeric researcher, Swerea KIMAB Klas.esbo@swerea.se

Example

• Clear damages was noted during inspection and a represented piece

was cut out

28

Possible to cut

out and repair?

Corrosion and cracks?

Change in

mechanical strength?

50% reduction!

Page 29: Handbook and damage atlas for inspection of glass fiber ... · Handbook and damage atlas for inspection of glass fiber reinforced plastics Polymeric researcher, Swerea KIMAB Klas.esbo@swerea.se

Example The Skoghall plant had problems with leaking

joints on their Anolyte line made of Alpolite (Viapal)

Potential service life of

20 years.

Poor joints reduced the

lifetime by a factor of 2.

Page 30: Handbook and damage atlas for inspection of glass fiber ... · Handbook and damage atlas for inspection of glass fiber reinforced plastics Polymeric researcher, Swerea KIMAB Klas.esbo@swerea.se

Conclusions

30

Page 31: Handbook and damage atlas for inspection of glass fiber ... · Handbook and damage atlas for inspection of glass fiber reinforced plastics Polymeric researcher, Swerea KIMAB Klas.esbo@swerea.se

Conclusions

• GRPs have a complex structure

• Many different failures and damages can occur. They are not always

dangerous.

• Inspections are very important. Damages can be hard to detect

• Calculations are difficult

31

Page 32: Handbook and damage atlas for inspection of glass fiber ... · Handbook and damage atlas for inspection of glass fiber reinforced plastics Polymeric researcher, Swerea KIMAB Klas.esbo@swerea.se

32

Scientific Work for Industrial Use

www.swerea.se