FRACTOGRAPHIC INVESTIGATION OF THE FAILURE OF SECOND … · construction [1]. Gas turbine blades...
Transcript of FRACTOGRAPHIC INVESTIGATION OF THE FAILURE OF SECOND … · construction [1]. Gas turbine blades...
![Page 1: FRACTOGRAPHIC INVESTIGATION OF THE FAILURE OF SECOND … · construction [1]. Gas turbine blades are critical components in power plants which in the event of their failure the power](https://reader034.fdocuments.us/reader034/viewer/2022050202/5f559ace2cad2e751d2bddab/html5/thumbnails/1.jpg)
8. Uluslar Aras K lma Konferans Bildiriler Kitab 7 – 9 Kas m 2007Prooceedings of 8th International Fracture Conference 7 – 9 November 2007
Istanbul/TURKEY
577
FRACTOGRAPHIC INVESTIGATION OF THE FAILUREOF SECOND STAGE GAS TURBINE BLADES
Hassan FARHANGI and Ali Asghar FOULADI MOGHADAM
School of Metallurgy and Materials Engineering, Faculty of Engineering,University of Tehran, Tehran, Iran.
ABSTRACT
This paper deals with a fracture investigation of second stage turbine blades in a 32 MW unitin a thermal power plant. The premature failure of the blades, made of nickel based superalloyUdimet 500, occurred after a service life of 50000 h and caused extensive damage to the unit.Several fractured blades were retrieved from the unit to identify the cause of failure. Theinvestigation included visual examination, SEM fractography, chemical analysis, hardnessmeasurement, and microstructural characterization. Detailed examinations of the bladesindicated that the primary failure event was related to the fracture of a turbine blade at the topfirtree root. The fracture surface morphology exhibited features characteristic of slow stablecrack growth by crystallographic faceted cracking and striation formation that was terminatedby interdendiritic fracture at the final stage of failure. These together with the results ofmacrofractographic observations identified high cycle fatigue as the primary contributingfracture mechanism. The main fatigue crack initiated on a surface that was damaged byfretting wear as evident from the debris on the contact surfaces of the firtree joint. Thephysical characteristics of fretting damage in relation to crack initiation are discussed basedon the microstructural and fractographic findings presented.
Keywords: Firtree joint, Fractography, Fretting fatigue, Turbine blade, Udimet 500.
1. INTRODUCTION
Gas turbine blades are made of nickel-base and cobalt-base superalloys principally. Duringthe past few decades, the operating temperatures of gas turbine engines have been on the riseto achieve higher and higher engine power and efficiency. This has necessitated a continuingadvancement in the temperature withstanding capabilities of materials used in theirconstruction [1]. Gas turbine blades are critical components in power plants which in theevent of their failure the power plants will shut down. This case can cause long time currentfailure and economic loss. Therefore, it is necessary to settle the failure analysis of turbineblades in order to increase the reliability of turbine systems [2,3].Turbine blades are susceptible to damage and crack formation in regions of componentcontact that experience both centrifugal and oscillatory vibrations [4]. A component subjectedto fatigue in the presence of mating component under a contact load experiences micro-slipalong the contacting interface, and causes a significant reduction in fatigue life. This iscommonly referred to as fretting fatigue that results in an increase in tensile and shear stressesat the contact surface, which acts as a damage generator leading to crack nucleation, growth,
![Page 2: FRACTOGRAPHIC INVESTIGATION OF THE FAILURE OF SECOND … · construction [1]. Gas turbine blades are critical components in power plants which in the event of their failure the power](https://reader034.fdocuments.us/reader034/viewer/2022050202/5f559ace2cad2e751d2bddab/html5/thumbnails/2.jpg)
8. Uluslar Aras K lma Konferans Bildiriler Kitab 7 – 9 Kas m 2007Prooceedings of 8th International Fracture Conference 7 – 9 November 2007
Istanbul/TURKEY
578
and eventually failure faster than that under the conventional fatigue condition withoutfretting (plain fatigue). The reduction in life of machine components under fretting fatigue ascompared to plain fatigue has been demonstrated by a number of researchers [1,2]. Theblade/disk attachment at the firtree joint, in gas turbine engines is one of critical componentswhich can fail due to fretting fatigue. This component is subjected to high cycle fatigue(HCF) condition that involves high frequencies and vibrational type loads often superimposedon a high mean stress [3-5].During the fretting fatigue process, cracks will nucleate and propagate according to severestress gradients that are generated from of the effective shape of contact, coefficient offriction, and the applied loads [1]. These fretting cracks are initially very small, but mayeventually lead to severe component damage [4]. Different signs have been introduced forfretting fatigue conditions which include: formation of wear products on contact surface andcrack opening, presence of wear track on contact surface, crack nucleation in vicinity of weartracks, micro plastic deformation in nucleation site and the slant orientation of crack in thenucleation region [6].This paper reports the fracture investigation of second stage turbine blades in a 32 MW unit ina thermal power plant. The premature failure of the blades occurred after a service life of50000 h and caused extensive damage to the unit. The primary failure event, which wasrelated to the fracture of a turbine blade at the firtree joint, under the influence of frettingfatigue conditions, is analyzed based on fractographic studies of crack initiation and growthon the turbine blade failure surface and physical characterization of fretting damage inrelation to crack nucleation.
2. EXPERIMENTAL METHODS
A damaged turbine blade which was retrieved from the accident site is shown in Figure 1. Thefirtree joint is also separately presented in the above mentioned figure. The remaining portionof the main fractured turbine blade under investigation which only includes the firtree rootregion, due to complete separation of the air foil section of the blade in the fracture process, isshown in Figure 2.
Figure 1. Blade geometry and the firtree joint of a damaged turbine blade.
airfoil
firtreejoint
leadingedge trailing
edge
![Page 3: FRACTOGRAPHIC INVESTIGATION OF THE FAILURE OF SECOND … · construction [1]. Gas turbine blades are critical components in power plants which in the event of their failure the power](https://reader034.fdocuments.us/reader034/viewer/2022050202/5f559ace2cad2e751d2bddab/html5/thumbnails/3.jpg)
8. Uluslar Aras K lma Konferans Bildiriler Kitab 7 – 9 Kas m 2007Prooceedings of 8th International Fracture Conference 7 – 9 November 2007
Istanbul/TURKEY
579
Figure 2. The remaining firtree root region of the fractured blade.
Following visual examination and digital camera photo documentation, portions of thefracture surface were cut for microfractographic studies by scanning electron microscopeequipped with an energy dispersive spectroscopy, EDS analysis facility. The specimens weresubjected to SEM examinations in the as received condition as well as following ultrasoniccleaning. All the specimens used for material characterization were prepared from locationsbeneath the fracture surface. Chemical analysis was carried out using optical emissionspectroscopy method. Specimen preparation for macroscopic and microscopic metallurgicalevaluations on longitudinal and transverse sections was carried out using standardmetallography techniques, followed by etching the specimens with Marbel reagent.Macrohardness measurements were performed using Rockwell C hardness testing method.
3. RESULTS AND DISCUSSION
3.1 Material characterizationChemical analysis was conducted using optical emission spectroscopy method on specimencut from the firtree root region beneath the fracture surface. The results of chemical analysisare shown in Table 1, which are in good agreement with the standard chemical compositionfor Udimet 500 superalloy [7].
Table 1. Chemical composition of turbine blade
Composition (wt. %)Source ofdata Ni Cr Co Mo Al Ti Ta C B
Chemicalanalysis 52.99 18.98 17.25 3.93 3.40 3.17 0.366 0.080 0.006
Udimet500 [7] 53 18 17 4 3 3 0.02 0.1 0.02
Metallographic observations were carried on transverse and longitudinal sections preparedfrom the firtree root region of the turbine blade beneath the fracture surface. A macroethedmetallographic section of the firtree root showing the coarse dendritic structure of the castUdimet 500 superalloy is presented in Figure 3(a). Distribution of fine gamma prime particlesand interdendritic carbides in the matrix can be seen in a higher magnification SEMmicrograph in Figure 3(b). The common strengthening mechanism of this alloy isprecipitation hardening through gamma prime precipitation in the matrix. The gamma primephase is an intermetallic compound of nominal composition [Ni3(Al,Ti)] which is stable overa relatively narrow range of composition. The morphology of the gamma prime particles inthe firtree root region does not seem to have been abnormally affected by the long termservice of the turbine blade. The average hardness number of the blade material was found tobe 32 HRC which was fairly uniform across the various metallographic sections.
top firtreeroot
![Page 4: FRACTOGRAPHIC INVESTIGATION OF THE FAILURE OF SECOND … · construction [1]. Gas turbine blades are critical components in power plants which in the event of their failure the power](https://reader034.fdocuments.us/reader034/viewer/2022050202/5f559ace2cad2e751d2bddab/html5/thumbnails/4.jpg)
8. Uluslar Aras K lma Konferans Bildiriler Kitab 7 – 9 Kas m 2007Prooceedings of 8th International Fracture Conference 7 – 9 November 2007
Istanbul/TURKEY
580
(a) (b)
Figure 3. (a) Macroetched section of the firtree root, (b) SEM micrograph showinggamma prime particles and interdendiritic carbides.
3.2 FractographyThe side view of the fractured blade presented in Figure 2 shows that the failure surface islocated at the top firtree root. The general orientation of the fracture surface is nearly normalto the longitudinal axis of the blade. Visual examination of the fractured blade indicates thatthe fracture process involved minimal gross plastic deformation with no visible sign of anychange in the cross section area at the fracture location. Thus the failure of the blade can beconsidered as a macroscopically brittle fracture process.Macroscopic appearance of the fracture surface is shown in Figure 4. Two distinct regionsdenoted as A and B, which is delineated by a curved superposed boundary line, can beidentified on the fracture surface. Region A has a more shiny appearance and extends fromthe boundary to the trailing edge side of the blade and covers about 40% of the fracturesurface. Region B located in the opposite side extends up to the leading edge side of the blade.The fracture mechanisms in these regions are analyzed by SEM fractography.
Figure 4. Fracture surface of the blade.
Following detailed SEM examinations of region A, a semielliptical crack region whichoriginated at the top firtree root was found as shown in Figure 5(a). Fine radial markingsemanating from the crack nucleation zone can be seen in this fractograph. The fracture surfaceappearance in the early stages of crack growth near the initiation site is shown in Figure 5(b).
fatigue region (A)
finalfracture
region (B)
10 m
![Page 5: FRACTOGRAPHIC INVESTIGATION OF THE FAILURE OF SECOND … · construction [1]. Gas turbine blades are critical components in power plants which in the event of their failure the power](https://reader034.fdocuments.us/reader034/viewer/2022050202/5f559ace2cad2e751d2bddab/html5/thumbnails/5.jpg)
8. Uluslar Aras K lma Konferans Bildiriler Kitab 7 – 9 Kas m 2007Prooceedings of 8th International Fracture Conference 7 – 9 November 2007
Istanbul/TURKEY
581
Faceted crystallographic crack growth characterizes the fracture surface morphology in thisregion. This type of crack growth has been previously reported for many planar slip and lowstacking fault energy FCC alloys, including many of the nickel based superalloys, undercyclic crack growth conditions at relatively low stress intensity amplitudes [2]. Furtherexamination of the fracture surface, in the middle parts of region A, reveals the formation oftypical striation markings characteristic of progressive crack growth under high cycle fatigueconditions [8]. A fine band of dense striations can be seen in Figure 5(c). The fracture surfacemorphology in region B is indicative of a distinctly different type of fracture mechanism. Theinterdendiritic and typically rough morphology of the fracture surface in this region is shownin Figure 5(d). This change in fracture surface morphology is associated with a transition fromstable cyclic crack growth to unstable fast fracture due to the exhaustion of the load carryingcapacity of the blade. From the fractographic point of view the change in fracture mode fromtransdendritic to interdendiritic is considered as one of the typical features of fracture of castmaterials by a fatigue mechanism.
(a) (b)
(c) (d)
Figure 5. SEM fractographs showing (a) semielliptical crack in the iniation region (b)crystallographic fatigue crack growth, (c) characteristic fatigue striations and (d)
interdendritic fracture morphology in the final fracture region.
A magnified view of the fatigue facture region of the turbine blade root failure surface isshown in Figure 6. The partially discolored region corresponds to the roughly thumb nail
250 m
10 m 500 m
1mm
![Page 6: FRACTOGRAPHIC INVESTIGATION OF THE FAILURE OF SECOND … · construction [1]. Gas turbine blades are critical components in power plants which in the event of their failure the power](https://reader034.fdocuments.us/reader034/viewer/2022050202/5f559ace2cad2e751d2bddab/html5/thumbnails/6.jpg)
8. Uluslar Aras K lma Konferans Bildiriler Kitab 7 – 9 Kas m 2007Prooceedings of 8th International Fracture Conference 7 – 9 November 2007
Istanbul/TURKEY
582
shape crack extending from the crack initiation zone and is indicative of the exposure of thecracked blade to gas flow process. Close examination of the contact surfaces of the firtreejoint reveals the formation of continuous tracks of about 3 mm wide across the entire contactsurfaces (Figure 6). The magnified morphology of the tracks is shown in a SEM micrographin Figure 7.
Figure 6. Magnified views of fatigue facture region and a wear track .
Figure 7. SEM micrograph of trapped debris forming a wear track.
initiation zone
wear track
discolored region
1000 m
![Page 7: FRACTOGRAPHIC INVESTIGATION OF THE FAILURE OF SECOND … · construction [1]. Gas turbine blades are critical components in power plants which in the event of their failure the power](https://reader034.fdocuments.us/reader034/viewer/2022050202/5f559ace2cad2e751d2bddab/html5/thumbnails/7.jpg)
8. Uluslar Aras K lma Konferans Bildiriler Kitab 7 – 9 Kas m 2007Prooceedings of 8th International Fracture Conference 7 – 9 November 2007
Istanbul/TURKEY
583
The tracks seem to consist of accumulated wear debris particles trapped between the contactsurfaces. EDS analysis of the wear debris shown in Figure 8 reveals a high concentration ofiron, which is the base element in the chemical composition of the Cr-Mo-V steel discmaterial.
Figure 8. EDS analysis of wear debris particles on the wear tracks.
This entrapment of wear debris normally occurs under fretting wear conditions whenopposing local surface regions in tightly held components undergo a small localized relativedisplacement for long periods. These conditions are typically encountered in the firtree rootsof the rotating turbine blades. The firtree roots are also subjected to vibratory loads and highcentrifugal forces leading to elevated contact and bulk stress, which combined with therelative displacements during operational cycles, compels them to endure fretting fatigueconditions. It can be seen from the magnified views of the crack initiation region and the weartracks shown in Figure 6 that crack initiation region is located in close proximity of the weartrack on the top firtree root. Furthermore the crack orientation in the initiation region is at aninclined angle with respect to the blade axis as shown in the SEM fractograph in Figure 9.
Figure 9. SEM micrograph showing slant crack orientation at the initiation region.
250 m
Element Weight%O K 18.31Al K 2.43Si K 4.07S K 1.29Ti K 1.82Cr K 6.94Fe K 34.56Co K 7.50Ni K 23.08Totals 100.00
![Page 8: FRACTOGRAPHIC INVESTIGATION OF THE FAILURE OF SECOND … · construction [1]. Gas turbine blades are critical components in power plants which in the event of their failure the power](https://reader034.fdocuments.us/reader034/viewer/2022050202/5f559ace2cad2e751d2bddab/html5/thumbnails/8.jpg)
8. Uluslar Aras K lma Konferans Bildiriler Kitab 7 – 9 Kas m 2007Prooceedings of 8th International Fracture Conference 7 – 9 November 2007
Istanbul/TURKEY
584
The above findings which include the formation of wear products on contact surfaces offirtree root, presence of wear tracks, crack nucleation in the vicinity of wear tracks and theslant orientation of the crack in the nucleation region are indicative of the strong influence ofthe fretting fatigue mechanism [9,10] on the failure of the blade under investigation.
4. CONCLUSIONS
1- Based on fractographic observations three distinct stages including, crack initiation, crackgrowth and final fracture were identified on the failure surface of the fractured blade whichhad failed at the top firtree root in the blade/disc joint.2- Formation of wear products on the contact surfaces of firtree root, presence of wear tracks,crack initiation in vicinity of wear tracks and the slant orientation of crack in the nucleationregion are indicative of primary contributions of fretting fatigue mechanism to the failureprocess of the blade.3- Stable cyclic crack growth regions by crystallographic faceted cracking and striationformation were identified on the fatigue fracture surface.4- The transition from stable cyclic crack growth to unstable fast fracture was accompaniedby a change from transdendritic to interdendiritic fracture mode.
ACKNOWLEDGEMENTSThe authors are grateful to Eng. S. Parsa of Ray Electric Power Production ManagementCompany, for his support and stimulating discussions. The authors also acknowledge thehelpful assistance of Eng. F. Hassanabadi during the study.
REFERENCES
1. Bhaumik S. K., Sujata M., “Failure of a low pressure turbine rotor blade of an aeroengine”, Journal ofEngineering Failure Analysis, Vol.13, pp. 1202-1219, 2006.
2. Wang W., Xuan F., “Failure analysis of the final stage blade in steam turbine”, Journal of EngineeringFailure Analysis, Vol.14, pp. 632-641, 2007.
3. Vardar N., Ekerim A., “Failure analysis of gas turbine blades in a thermal power plant”, Journal ofEngineering Failure Analysis, Vol.14, pp. 743-749, 2007.
4. Garcia D.B., Grandt A.F., “Fractographic investigation of fretting fatigue cracks in Ti–6Al–4V”,Journal of Engineering Failure Analysis, Vol.12, pp. 537–548, 2005.
5. Mall S., Namjoshi S.A., Porter W.J., “Effects of microstructure on fretting fatigue crack initiationbehavior of Ti-6Al-4V”, Journal of Materials Science and Engineering, Vol.383, pp. 334–340, 2004.
6. Nowell D., Dini D., Hills D.A., “Recent developments in the understanding of fretting fatigue”, Journalof Engineering Fracture Mechanics, Vol.73, pp. 207-222, 2006.
7. ASM, Metals Handbook: Properties and Selection, Vol. 2, 10th ed., Materials Park, OH, pp. 436-444, 1990.
8. Brooks C. R., Metallurgical Failure Analysis, McGraw-Hill, New York, USA, pp. 140-170, 1993.9. Rajasekaran R., Nowell D., “Fretting fatigue in dovetail blade roots: Experiment and analysis”, Journal
of Tribology International, Vol.39, pp. 1277–1285, 2006.10. Jin O., Mall S., “Effects of slip on fretting behavior: experiments and analyses”, Journal of Wear,
Vol.256, pp. 671–684, 2004.