Flexible and efficient hydrometallurgical recycling of Li-ion … · 2020. 12. 17. ·...
Transcript of Flexible and efficient hydrometallurgical recycling of Li-ion … · 2020. 12. 17. ·...
![Page 1: Flexible and efficient hydrometallurgical recycling of Li-ion … · 2020. 12. 17. · •Challenge: The. presence of polyvinylidene fluoride (PVDF)- the binder for the active material](https://reader036.fdocuments.us/reader036/viewer/2022071608/6145d7a88f9ff812541fe211/html5/thumbnails/1.jpg)
Flexible and efficient hydrometallurgical recycling of Li-ion batteries of different chemistry
Gabriele LombardoPhD Student
![Page 2: Flexible and efficient hydrometallurgical recycling of Li-ion … · 2020. 12. 17. · •Challenge: The. presence of polyvinylidene fluoride (PVDF)- the binder for the active material](https://reader036.fdocuments.us/reader036/viewer/2022071608/6145d7a88f9ff812541fe211/html5/thumbnails/2.jpg)
Scheme of a Lithium Battery
LiCoO2LiMn2OLiNiO2
![Page 3: Flexible and efficient hydrometallurgical recycling of Li-ion … · 2020. 12. 17. · •Challenge: The. presence of polyvinylidene fluoride (PVDF)- the binder for the active material](https://reader036.fdocuments.us/reader036/viewer/2022071608/6145d7a88f9ff812541fe211/html5/thumbnails/3.jpg)
Dismantling
![Page 4: Flexible and efficient hydrometallurgical recycling of Li-ion … · 2020. 12. 17. · •Challenge: The. presence of polyvinylidene fluoride (PVDF)- the binder for the active material](https://reader036.fdocuments.us/reader036/viewer/2022071608/6145d7a88f9ff812541fe211/html5/thumbnails/4.jpg)
Mechanical pre-treatment
4
Current state of Li-ion batteries recycling
Pyrometallurgical treatment Hydrometallurgical treatment
Li
slag
![Page 5: Flexible and efficient hydrometallurgical recycling of Li-ion … · 2020. 12. 17. · •Challenge: The. presence of polyvinylidene fluoride (PVDF)- the binder for the active material](https://reader036.fdocuments.us/reader036/viewer/2022071608/6145d7a88f9ff812541fe211/html5/thumbnails/5.jpg)
List of critical raw materials for EU - 2017
![Page 6: Flexible and efficient hydrometallurgical recycling of Li-ion … · 2020. 12. 17. · •Challenge: The. presence of polyvinylidene fluoride (PVDF)- the binder for the active material](https://reader036.fdocuments.us/reader036/viewer/2022071608/6145d7a88f9ff812541fe211/html5/thumbnails/6.jpg)
Forecasts of global electric vehicle sales by 2030
SOURCE: BLOOMBERG NEW ENERGY FINANCE
![Page 7: Flexible and efficient hydrometallurgical recycling of Li-ion … · 2020. 12. 17. · •Challenge: The. presence of polyvinylidene fluoride (PVDF)- the binder for the active material](https://reader036.fdocuments.us/reader036/viewer/2022071608/6145d7a88f9ff812541fe211/html5/thumbnails/7.jpg)
3. Leaching
4. Solvent extraction
1. Pyrolysis
2. Mechanical Separation
Steps of the process being developed at Chalmers:
![Page 8: Flexible and efficient hydrometallurgical recycling of Li-ion … · 2020. 12. 17. · •Challenge: The. presence of polyvinylidene fluoride (PVDF)- the binder for the active material](https://reader036.fdocuments.us/reader036/viewer/2022071608/6145d7a88f9ff812541fe211/html5/thumbnails/8.jpg)
• Challenge:
The presence of polyvinylidene fluoride (PVDF)- the binder for the active material to be attached with the current collectors (thin copper and aluminium foils).
• It affects: 1. The mechanical separation process in which it obstructs the separation of the active material and
carbon (also called black mass) from the foils.2. The leaching process in which it prevents the contact of the leaching media with the material.
• Solution: Removal of PVDF by thermal methods (pyrolysis or incineration).
• Benefit: Utilization of carbon.
Pyrolysis
![Page 9: Flexible and efficient hydrometallurgical recycling of Li-ion … · 2020. 12. 17. · •Challenge: The. presence of polyvinylidene fluoride (PVDF)- the binder for the active material](https://reader036.fdocuments.us/reader036/viewer/2022071608/6145d7a88f9ff812541fe211/html5/thumbnails/9.jpg)
Pyrolysis
Carbon Metal oxides
Li,Co,Mn, NiCO2 and CO
+
+
Pyrolysis
![Page 10: Flexible and efficient hydrometallurgical recycling of Li-ion … · 2020. 12. 17. · •Challenge: The. presence of polyvinylidene fluoride (PVDF)- the binder for the active material](https://reader036.fdocuments.us/reader036/viewer/2022071608/6145d7a88f9ff812541fe211/html5/thumbnails/10.jpg)
Analysis of the unaltered batteryLiquid fraction (ICP analysis)
Cathode AnodeConc. (ppm) %W Conc. (ppm) %W
Al 282.4 7.06 0,8 0.00Co 233.0 5.83 0 0.00Cu 0 0.00 1417.5 35.44K 3.4 0.09 2,8 0.07Li 106.5 2.66 4.768 0.12
Mn 664.3 16.61 -Ni 228.4 5.71 0.14 0.089Si 2.9 0.07 2.7 0.07
Cathode AnodeConc. (ppm) %W Conc. (ppm) %W
Al 282.4 7.06 0,8 0.00Co 233.0 5.83 0 0.00Cu 0 0.00 1417.5 35.44K 3.4 0.09 2,8 0.07Li 106.5 2.66 4.768 0.12
Mn 664.3 16.61 -Ni 228.4 5.71 0.14 0.089Si 2.9 0.07 2.7 0.07
Analyzed elements
Li Co Cr Cu Al Mn Ni K Mo Si Y Na Fe Sn Mg
![Page 11: Flexible and efficient hydrometallurgical recycling of Li-ion … · 2020. 12. 17. · •Challenge: The. presence of polyvinylidene fluoride (PVDF)- the binder for the active material](https://reader036.fdocuments.us/reader036/viewer/2022071608/6145d7a88f9ff812541fe211/html5/thumbnails/11.jpg)
Setting of the process:
• Temperature: 400ºC, 500ºC, 600ºC, 700ºC.
• Time: 30 min, 1h, 1.5h.
• Flow of nitrogen: around 340 ml/min.
Pyrolysis
![Page 12: Flexible and efficient hydrometallurgical recycling of Li-ion … · 2020. 12. 17. · •Challenge: The. presence of polyvinylidene fluoride (PVDF)- the binder for the active material](https://reader036.fdocuments.us/reader036/viewer/2022071608/6145d7a88f9ff812541fe211/html5/thumbnails/12.jpg)
Variation of the weight of the samples before and after the thermal treatment.
The thermal treatment causes a variation of weight of the sample that is due by the formation ofvolatile species: the oxidation of graphite and other organic compound. The variation increased withthe rise of temperature and time.
Pyrolysis 400 500 600 700
30 min 1h 1.5 h 30 min 1h 1.5 h 30 min 1h 1.5 h 30 min 1h 1.5 h
Average delta % 6.89 9.17 11.28 9.26 11.90 15.65 9.32 12.51 18.94 11.40 15.54 22.18
![Page 13: Flexible and efficient hydrometallurgical recycling of Li-ion … · 2020. 12. 17. · •Challenge: The. presence of polyvinylidene fluoride (PVDF)- the binder for the active material](https://reader036.fdocuments.us/reader036/viewer/2022071608/6145d7a88f9ff812541fe211/html5/thumbnails/13.jpg)
By-productsWhite gas Oil (TAR)
![Page 14: Flexible and efficient hydrometallurgical recycling of Li-ion … · 2020. 12. 17. · •Challenge: The. presence of polyvinylidene fluoride (PVDF)- the binder for the active material](https://reader036.fdocuments.us/reader036/viewer/2022071608/6145d7a88f9ff812541fe211/html5/thumbnails/14.jpg)
etc
The formation of smoke happens in particular during the first 5-10 minutes of heating
It is possible that the smoke is produced by: Oxidation of the organic speces with formation of CO and CO2
the process of decomposition of PVDF that produces HF in gas phase.
Ftir analysis
Gas off analysis
![Page 15: Flexible and efficient hydrometallurgical recycling of Li-ion … · 2020. 12. 17. · •Challenge: The. presence of polyvinylidene fluoride (PVDF)- the binder for the active material](https://reader036.fdocuments.us/reader036/viewer/2022071608/6145d7a88f9ff812541fe211/html5/thumbnails/15.jpg)
Ftir analysis: CathodeComparison between a spectra in absorbance of a sample treated at 600°C per 2 and 5 minutes.
CO2
CO
HF
H2O
![Page 16: Flexible and efficient hydrometallurgical recycling of Li-ion … · 2020. 12. 17. · •Challenge: The. presence of polyvinylidene fluoride (PVDF)- the binder for the active material](https://reader036.fdocuments.us/reader036/viewer/2022071608/6145d7a88f9ff812541fe211/html5/thumbnails/16.jpg)
Ftir analysisCathode
• The peaks of the CO2 and CO are really intense, especially for the samples treated per 5 minutes. The oxidation of the carbon is due to the reaction with the metal salts present in the active material during the pyrolysis.
• C-F and H-F bond, whose presence is caused by the decomposition of the PVDF: the concentration of fluorides seems much more presence in the first minutes.
• Water vapor.
• Presence of organics specie as ketone and ester. The most probable origin has to be found in the evaporation of the electrolyte.
Anode
• The peaks for CO2 and CO, higher than in the cathode. There is a decreasing of the quantity of this specie in the gas off with time.
• Water vapor.
![Page 17: Flexible and efficient hydrometallurgical recycling of Li-ion … · 2020. 12. 17. · •Challenge: The. presence of polyvinylidene fluoride (PVDF)- the binder for the active material](https://reader036.fdocuments.us/reader036/viewer/2022071608/6145d7a88f9ff812541fe211/html5/thumbnails/17.jpg)
Mechanical Separation: Removal of black mass
Separation of black mass from aluminum and copper foils.
Improved purity of input material for hydrometallurgical treatment.
Simplification of solvent extraction process and decreasing of the energy demands for recovery of copper and aluminum.
![Page 18: Flexible and efficient hydrometallurgical recycling of Li-ion … · 2020. 12. 17. · •Challenge: The. presence of polyvinylidene fluoride (PVDF)- the binder for the active material](https://reader036.fdocuments.us/reader036/viewer/2022071608/6145d7a88f9ff812541fe211/html5/thumbnails/18.jpg)
Mechanical Separation: Removal of black mass
a b
a) sample holder of a ball mill; b) rotation plate with holders.
Setting of the process:
• Sample treated for 1.5 h at 600-700C.• Pieces of 16 cm2.• 10 minutes in the ball mill at 600 rpm.
The same treatment were applied on untreated samples in order to evaluate the efficiency. At the end of the rotation the powder was separated from the solid and weight.
![Page 19: Flexible and efficient hydrometallurgical recycling of Li-ion … · 2020. 12. 17. · •Challenge: The. presence of polyvinylidene fluoride (PVDF)- the binder for the active material](https://reader036.fdocuments.us/reader036/viewer/2022071608/6145d7a88f9ff812541fe211/html5/thumbnails/19.jpg)
Mechanical Separation: Removal of black mass
Thermal treatment followed by a mechanical one permit a separation of graphite and black mass from the metal layers with an efficiency of the 70%.
This is probably due to a decomposition at high temperature of the polymers as PVDF that working as glue between the metals layers and the active material.
The hydrometallurgical process can be significantly simplify.
TreatedUntreated
TreatedUntreated
![Page 20: Flexible and efficient hydrometallurgical recycling of Li-ion … · 2020. 12. 17. · •Challenge: The. presence of polyvinylidene fluoride (PVDF)- the binder for the active material](https://reader036.fdocuments.us/reader036/viewer/2022071608/6145d7a88f9ff812541fe211/html5/thumbnails/20.jpg)
XRD analysis and Thermodynamic consideration
![Page 21: Flexible and efficient hydrometallurgical recycling of Li-ion … · 2020. 12. 17. · •Challenge: The. presence of polyvinylidene fluoride (PVDF)- the binder for the active material](https://reader036.fdocuments.us/reader036/viewer/2022071608/6145d7a88f9ff812541fe211/html5/thumbnails/21.jpg)
Pyrolysis : XRD analysis
It was observed:
• The presence of metals in elemental form, as Li, Ni, Mn, Cu and Co.
• Mn3O4, Al2O3: aluminum and manganese react as reductant agents with the other metals.
• Li2O: lithium is extremely reactive and its oxidation is thermodynamically favorite at the conditions of the process.
• Increasing of the treatment temperature determines a decreasing of the quantity of the carbon in the sample.
![Page 22: Flexible and efficient hydrometallurgical recycling of Li-ion … · 2020. 12. 17. · •Challenge: The. presence of polyvinylidene fluoride (PVDF)- the binder for the active material](https://reader036.fdocuments.us/reader036/viewer/2022071608/6145d7a88f9ff812541fe211/html5/thumbnails/22.jpg)
Pyrolysis
It is possible have an idea of the variation in quantity of carbon, analyzing the XRD spectra of samples treated at different temperature.
The 26.5°, 44.8° and 54.9° peaks were identified as originated by the graphitic carbon present on the anode: the green curve (700°C) is much low then the others.
![Page 23: Flexible and efficient hydrometallurgical recycling of Li-ion … · 2020. 12. 17. · •Challenge: The. presence of polyvinylidene fluoride (PVDF)- the binder for the active material](https://reader036.fdocuments.us/reader036/viewer/2022071608/6145d7a88f9ff812541fe211/html5/thumbnails/23.jpg)
Pyrolysis : XRD analysis
LiCoO2
The XRD spectra shows the presence of Li2O, CoO2, Co3O4, CoO and Co, these last two has a stronger signals compared to the others.
1. 4LiCoO2(s) + 3 C(s) = 2 Li2O(s) + 4 Co(s) + 3 CO2(g)
2. 2LiCoO2 +3 CO(g) = Li2O + 2Co + 3CO2(g)
3. 4LiCoO2 + C = 2Li2O + 4CoO + CO2(g)
![Page 24: Flexible and efficient hydrometallurgical recycling of Li-ion … · 2020. 12. 17. · •Challenge: The. presence of polyvinylidene fluoride (PVDF)- the binder for the active material](https://reader036.fdocuments.us/reader036/viewer/2022071608/6145d7a88f9ff812541fe211/html5/thumbnails/24.jpg)
Pyrolysis : XRD analysis
LiMn2O4The XRD spectra shows the presence of the presence of Li2O, Li, Mn3O4 and Mn.
The reactions studied are:
1. LiMnO4 + 2C = Li + Mn + 2CO2(g)2. LiMnO4 + 4CO(g) = Li + Mn + 4CO2(g)3. 3LiMnO4 + 4C = 3Li + Mn3O4 + 4CO2(g)4. 3LiMnO4 + 8CO(g) = 3Li + Mn3O4 + 8CO2(g)5. 3LiMnO4 + 3,25C = 1,5Li2O + Mn3O4 + 3,25CO2(g)6. 3LiMnO4 + 6,5CO(g) = 1,5Li2O + Mn3O4 + 6,5CO2(g)7. 2LiMnO4 + 3,5C = Li2O + 2Mn + 3,5CO2(g)8. 2LiMnO4 + 7CO(g) = Li2O + 2Mn + 7CO2(g)
T (°C)ΔG (kJ/mol)
1 2 3 4 5 6 7 8300 -137,78 -279,65 -810,95 -1094,70 -1302,06 -1532,60 -602,96 -851,24400 -174,10 -280,21 -885,93 -1098,15 -1355,71 -1528,14 -661,38 -847,08500 -212,27 -282,77 -966,66 -1107,67 -1415,16 -1529,73 -723,53 -846,91600 -252,07 -287,15 -1052,50 -1122,64 -1479,82 -1536,81 -789,03 -850,40700 -293,36 -293,20 -1142,93 -1142,60 -1549,23 -1548,97 -857,59 -857,31800 -336,21 -301,01 -1237,54 -1167,13 -1623,04 -1565,83 -929,43 -867,82
![Page 25: Flexible and efficient hydrometallurgical recycling of Li-ion … · 2020. 12. 17. · •Challenge: The. presence of polyvinylidene fluoride (PVDF)- the binder for the active material](https://reader036.fdocuments.us/reader036/viewer/2022071608/6145d7a88f9ff812541fe211/html5/thumbnails/25.jpg)
Pyrolysis : XRD analysis
LiNiO2
1. 2LiNiO2 +3 CO(g) = Li2O + 2Ni + 3CO2(g)2. 4LiNiO2 + C = 2Li2O + 4NiO + CO2(g)
The XRD spectra shows the presence of Li2O, Li, NiO and Ni.
ConclusionIn conclusion, the thermodynamic considerations show that the reactions between graphite, the reductive atmosphere present in the system and the salts in the black mass are spontaneous in the conditions of the process and their ΔG become more negative increasing the temperature.
![Page 26: Flexible and efficient hydrometallurgical recycling of Li-ion … · 2020. 12. 17. · •Challenge: The. presence of polyvinylidene fluoride (PVDF)- the binder for the active material](https://reader036.fdocuments.us/reader036/viewer/2022071608/6145d7a88f9ff812541fe211/html5/thumbnails/26.jpg)
Leaching and Solvent Extraction
![Page 27: Flexible and efficient hydrometallurgical recycling of Li-ion … · 2020. 12. 17. · •Challenge: The. presence of polyvinylidene fluoride (PVDF)- the binder for the active material](https://reader036.fdocuments.us/reader036/viewer/2022071608/6145d7a88f9ff812541fe211/html5/thumbnails/27.jpg)
Leaching - Several parameters such as different leaching agents, temperature, and solid to liquid ration are
studied in the leaching process. The aim is to develop efficient and more environmentally friendly leaching
procedure applicable for Li-ion batteries based on different chemistries.
Solvent extraction process: In the process of metal ions recovery different extractants are used to determine
optimal parameters flexible for differences in the leachates coming from previous step.
The developed processes will be scaled up in pilot scale leaching reactors and mixer settlers.
Leaching
Solvent extraction
![Page 28: Flexible and efficient hydrometallurgical recycling of Li-ion … · 2020. 12. 17. · •Challenge: The. presence of polyvinylidene fluoride (PVDF)- the binder for the active material](https://reader036.fdocuments.us/reader036/viewer/2022071608/6145d7a88f9ff812541fe211/html5/thumbnails/28.jpg)
Leaching
Cobalt leaching after thermal treatment: Lithium leaching after thermal treatment:
1M HCl – no reduction agent
![Page 29: Flexible and efficient hydrometallurgical recycling of Li-ion … · 2020. 12. 17. · •Challenge: The. presence of polyvinylidene fluoride (PVDF)- the binder for the active material](https://reader036.fdocuments.us/reader036/viewer/2022071608/6145d7a88f9ff812541fe211/html5/thumbnails/29.jpg)
Extraction (Mn) CYANEX 272/572 in kerosene Raffinate (Li, Co, Ni)
Scrubbing Scrubbing product (Mn, Ni)
Stripping
Extraction (Ni) raffinate (Li)
Stripping stripping product (Ni)
Li precipitationNa2CO3
MnCl2
HCl Stripping product ( Mn)
HCl
Li2CO3
CYANEX 272/572 in kerosene
Solid/ Liquid separation
Feed
Co precipitationNaClO
Co2O3Solid/ Liquid separation
Raffinate (Li, Ni)
![Page 30: Flexible and efficient hydrometallurgical recycling of Li-ion … · 2020. 12. 17. · •Challenge: The. presence of polyvinylidene fluoride (PVDF)- the binder for the active material](https://reader036.fdocuments.us/reader036/viewer/2022071608/6145d7a88f9ff812541fe211/html5/thumbnails/30.jpg)
Extraction (Mn) CYANEX 272/572 in kerosene Raffinate (Li, Co, Ni)
Scrubbing Scrubbing product (Mn, Ni)
Stripping
MnCl2
HCl Stripping product ( Mn)
Feed
![Page 31: Flexible and efficient hydrometallurgical recycling of Li-ion … · 2020. 12. 17. · •Challenge: The. presence of polyvinylidene fluoride (PVDF)- the binder for the active material](https://reader036.fdocuments.us/reader036/viewer/2022071608/6145d7a88f9ff812541fe211/html5/thumbnails/31.jpg)
Co precipitationNaClO
Co2O3Solid/ Liquid separation
Raffinate (Li, Ni)
![Page 32: Flexible and efficient hydrometallurgical recycling of Li-ion … · 2020. 12. 17. · •Challenge: The. presence of polyvinylidene fluoride (PVDF)- the binder for the active material](https://reader036.fdocuments.us/reader036/viewer/2022071608/6145d7a88f9ff812541fe211/html5/thumbnails/32.jpg)
Extraction (Ni) raffinate (Li)
Stripping stripping product (Ni)HCl
CYANEX 272/572 in kerosene
![Page 33: Flexible and efficient hydrometallurgical recycling of Li-ion … · 2020. 12. 17. · •Challenge: The. presence of polyvinylidene fluoride (PVDF)- the binder for the active material](https://reader036.fdocuments.us/reader036/viewer/2022071608/6145d7a88f9ff812541fe211/html5/thumbnails/33.jpg)
Li precipitationNa2CO3
Li2CO3Solid/ Liquid separation
![Page 34: Flexible and efficient hydrometallurgical recycling of Li-ion … · 2020. 12. 17. · •Challenge: The. presence of polyvinylidene fluoride (PVDF)- the binder for the active material](https://reader036.fdocuments.us/reader036/viewer/2022071608/6145d7a88f9ff812541fe211/html5/thumbnails/34.jpg)
S t o c k s o l u t i o n : M n C l 2 , C o C l 2 , N i C l 2 , L i C l i n H C l .S o l i d - l i q u i d r a t i o : 1 / 5 0 .T h e e f f i c i e n c y o f 2 a c i d i c e x t r a c t a n t s w a s c o m p e r e d : C y a n e x 2 7 2 a n d C y a n e x 5 7 2 , b o t h a t1 M .
T h e r e s u l t s r e p r e s e n t t h e v a l u e s o b t a i n e d a t p H e q u i l i b r i u m .
• T h e d i f f e r e n c e b e t w e e n t h e 2 e x t r a c t a n t s i s n o t s i g n i f i c a n t .
• L i r e m a i n s i n t h e a q u e o u s p h a s e t h r o u g h o u t t h e p H r a n g e i n v e s t i g a t e d a n d f o r b o t hC y a n e x 2 7 2 a n d 5 7 2 . T h i s g a v e a s t h e p o s s i b i l i t y t o r e c o v e r t h a t b y p r e c i p i t a t i o n .
• N i r e m a n s i n t h e h y d r o c h l o r i c a c i d s o l u t i o n a t p H 6 , i n s t e a d C o a n d M n r e s u l t e da l r e a d y p a r t i a l l y e x t r a c t e d i n o r g a n i c p h a s e a t p H 4 .
Solvent Extraction
![Page 35: Flexible and efficient hydrometallurgical recycling of Li-ion … · 2020. 12. 17. · •Challenge: The. presence of polyvinylidene fluoride (PVDF)- the binder for the active material](https://reader036.fdocuments.us/reader036/viewer/2022071608/6145d7a88f9ff812541fe211/html5/thumbnails/35.jpg)
http://www.circularmaterialsconference.se/
![Page 36: Flexible and efficient hydrometallurgical recycling of Li-ion … · 2020. 12. 17. · •Challenge: The. presence of polyvinylidene fluoride (PVDF)- the binder for the active material](https://reader036.fdocuments.us/reader036/viewer/2022071608/6145d7a88f9ff812541fe211/html5/thumbnails/36.jpg)
www.ceb2018.org
Circular Economy of Battery Production and Recycling
Gothenburg, 24-26th of September 2018
![Page 37: Flexible and efficient hydrometallurgical recycling of Li-ion … · 2020. 12. 17. · •Challenge: The. presence of polyvinylidene fluoride (PVDF)- the binder for the active material](https://reader036.fdocuments.us/reader036/viewer/2022071608/6145d7a88f9ff812541fe211/html5/thumbnails/37.jpg)
37
Thank you for your attention!
for more information contact:
Matina Patranikova:[email protected]
Gabriele Lombardo: [email protected]
![Page 38: Flexible and efficient hydrometallurgical recycling of Li-ion … · 2020. 12. 17. · •Challenge: The. presence of polyvinylidene fluoride (PVDF)- the binder for the active material](https://reader036.fdocuments.us/reader036/viewer/2022071608/6145d7a88f9ff812541fe211/html5/thumbnails/38.jpg)
Solvent Extraction and Precipitation
•Mn recovered by precipitation by drop-wise adding 0.5 mol L of 1 KMnO4 solution to leaching liquor, pH 2.
•Cyanex 572 or 272: separation of cobalt and nickel from Li.
•Na2CO3 to precipitate Li as LiCO3
•Co recovered by oxidative precipitation with NaClO at pH 3.
•Ni recovered by precipitation with sodium hydroxide to achieve pH 11 in a second step.
![Page 39: Flexible and efficient hydrometallurgical recycling of Li-ion … · 2020. 12. 17. · •Challenge: The. presence of polyvinylidene fluoride (PVDF)- the binder for the active material](https://reader036.fdocuments.us/reader036/viewer/2022071608/6145d7a88f9ff812541fe211/html5/thumbnails/39.jpg)
Aims of the project• Study the possibilities of removal of organic compounds from spent lithium ion
accumulators through thermal pre treatment.
• Study how the pyrolysis and combustion affects chemical and phase composition of the material.
• Characterization of by-products (off-gas, tar, etc.).
• Study the possibilities to separate electrode foils from active material.
• Development of hydrometallurgical technology for a metal recovery from spent LiB with emphasis to accommodate the process to the different chemistries of LiB.
• Testing the proposed technology in a pilot plant scale equipment to simulate conditions expected in a real plant scale.
![Page 40: Flexible and efficient hydrometallurgical recycling of Li-ion … · 2020. 12. 17. · •Challenge: The. presence of polyvinylidene fluoride (PVDF)- the binder for the active material](https://reader036.fdocuments.us/reader036/viewer/2022071608/6145d7a88f9ff812541fe211/html5/thumbnails/40.jpg)
![Page 41: Flexible and efficient hydrometallurgical recycling of Li-ion … · 2020. 12. 17. · •Challenge: The. presence of polyvinylidene fluoride (PVDF)- the binder for the active material](https://reader036.fdocuments.us/reader036/viewer/2022071608/6145d7a88f9ff812541fe211/html5/thumbnails/41.jpg)
Dismantling
Lithium battery cell SPA The weight of the entire cell is 480 g, it is composed by 19 layers of copper and 18 layers of aluminum and the plastic cover weight 23g.
single layer all layer % weight
Anode layer of copper 3.02 ±0.04 g 57.1 g 11.9
black mass 6.10 ±0.2 g 115.9 g 24.2
Cathode
layer of aluminum 2 ± 0.2 g 36.3 g 7.5 black mass 11.8 ±1 g 212.4 g 44.2
separator 2.33 ± 0.03 g 42.2 g 8.8
![Page 42: Flexible and efficient hydrometallurgical recycling of Li-ion … · 2020. 12. 17. · •Challenge: The. presence of polyvinylidene fluoride (PVDF)- the binder for the active material](https://reader036.fdocuments.us/reader036/viewer/2022071608/6145d7a88f9ff812541fe211/html5/thumbnails/42.jpg)
• Equal number of cathodes and anodes to obtain homogeneus samples.
• Dissolution in aqua regia (80ºC; 5h).
• Filtration Liquid fraction (ICP analysis)
Undissolved fraction (XRD analysis)
Analysis of the unaltered battery
![Page 43: Flexible and efficient hydrometallurgical recycling of Li-ion … · 2020. 12. 17. · •Challenge: The. presence of polyvinylidene fluoride (PVDF)- the binder for the active material](https://reader036.fdocuments.us/reader036/viewer/2022071608/6145d7a88f9ff812541fe211/html5/thumbnails/43.jpg)
Analysis of the unaltered batteryUndissolved fraction (XRD analysis)
Average %w undissolved fraction 20.8%
• Cathode : polymers that constitute the separator, PVDF,Al2O3.
• Anode shows that the undissolved material is constituted essentially by graphite.
![Page 44: Flexible and efficient hydrometallurgical recycling of Li-ion … · 2020. 12. 17. · •Challenge: The. presence of polyvinylidene fluoride (PVDF)- the binder for the active material](https://reader036.fdocuments.us/reader036/viewer/2022071608/6145d7a88f9ff812541fe211/html5/thumbnails/44.jpg)
ICP analysis
![Page 45: Flexible and efficient hydrometallurgical recycling of Li-ion … · 2020. 12. 17. · •Challenge: The. presence of polyvinylidene fluoride (PVDF)- the binder for the active material](https://reader036.fdocuments.us/reader036/viewer/2022071608/6145d7a88f9ff812541fe211/html5/thumbnails/45.jpg)
0
100
200
300
400
500
600
30 min 1 h 1.5 h
ppm
t
Mn
400 C500 C600C700 C
0
50
100
150
200
250
300
350
30 min 1 h 1.5 h
ppm
t
Ni 400
500
600
700
0
50
100
150
200
250
300
30 min 1 h 1.5 h
ppm
t
Co
400
500
600
700
0
20
40
60
80
100
120
140
30 min 1 h 1.5 h
ppm
t
Li 400
500
600
700
Graphic representation of the concentration in ppm of the element detected in the acid solutions obtained dissolving the samples pyrolyzed at different temperature and time
Pyrolysis: ICP analysis
The relative abundance of each element increase between 60% ( Cu, Ni) an 100% ( Mn, Co, Li, Al).
![Page 46: Flexible and efficient hydrometallurgical recycling of Li-ion … · 2020. 12. 17. · •Challenge: The. presence of polyvinylidene fluoride (PVDF)- the binder for the active material](https://reader036.fdocuments.us/reader036/viewer/2022071608/6145d7a88f9ff812541fe211/html5/thumbnails/46.jpg)
0
200
400
600
800
30 min 1 h
ppm
t
Mn 400 C
500 C
600 C
700 C
0
100
200
300
400
500
30 min 1 h
ppm
t
Ni 400 C
500 C
600 C
700 C
0
100
200
300
30 min 1 h
ppm
t
Co 400 C
500 C
600 C
700 C
0
50
100
150
200
30 min 1 h
ppm
t
Li 400 C
500 C
600 C
700 C
Graphic representation of the concentration in ppm of the elements detected in the acid solutions obtained dissolving the samples thermal treated at different temperature and time.
Combustion : ICP analysis