Objective
The objective of this experiment is :
1. To understand the stage that is involved in the creep test.
2. To experimentally obtain the creep curve.
3. To identify the properties of material while subjected to a tensile load.
4. To measure the rate of deformation of the material to stress at a constant temperature.
Theory
Creep is defined as time-dependent plastic deformation (elongation) of the metal at a
constant tensile load. It is also defined as high temperature progressive deformation at constant
stress. "High temperature" is a relative term dependent upon the materials involved. Creep rates
are used in evaluating materials for boilers, gas turbines, jet engines, ovens, or any application
that involves high temperatures under load. Understanding high temperature behavior of metals
is useful in designing failure resistant systems. A creep test can be studied by measuring the
permanent extension, after various time intervals, of test-pieces maintained at a constant
temperature. Measurements of strain are then recorded over a period of time as in Figure 1. After
the initial instantaneous extension, it shows that creep occurs in three stages :
Stage 1 (Primary creep) : This stage occurs at the beginning of the tests, and creep is
mostly transiently, not at a steady rate. Resistance to creep increases until stage 2 (secondary
creep) is reached.
Stage 2 (Secondary creep) : The rate of creep becomes roughly steady. This stage is often
referred to as steady state creep.
Stage 3 (Tertiary creep) : The creep rate begins to accelerate as the cross sectional area of
the specimen decreases due to necking or internal voiding decreases the effective area of the
specimen. If stage 3 is allowed to proceed, fracture will occur.
In many cases, the three parts of the curve are not clearly distinguishable. To obtain a
complete picture of the creep properties of a material, it is necessary to construct creep curves for
a range of stresses over a range of temperature. Such curves as shown in Figure 2 usually show
that, as the applied stress decreased the primary creep is also decreases, secondary creep is
prolonged, and the possible extension during tertiary creep tends to increase. Very low applied
stress may mean that tertiary creep dies not occur even after lengthy service life.
![Page 2: CREEP TEST COMPLETE.pdf](https://reader035.fdocuments.us/reader035/viewer/2022072922/54619533b1af9f936c8b49b9/html5/thumbnails/2.jpg)
Specimen and Equipment
1. Creep measurement apparatus
2. Vernier caliper
3. Stopwatch
4. Specimens - plastic
Procedures
1. The original gauge length, thickness and width of the gauge length of the specimen was
measured and recorded in the table.
2. Then, the maximum load that can be stand by the specimen was measured .
3. The force that lower than maximum load of the specimen was used in the creep test.
4. After that, specimen was placed to the creep test machine to obtain the result
5. The force-time graph of creep test been observed on the monitor of the test’s equipment
6. Step 3 until 5 was repeated until the typical creep curve of strain versus time at constant
stress was obtained
7. When the typical creep curve of strain versus time at constant stress was obtained, the
machine was been stopped.
8. The result and graph obtained had been saved and recorded.
9. Analysis had been done.
Figure 1 : Typical creep curve of strain
versus time at constant stress and
elevated temperature
Figure 2 : Influence of stress σ and
temperature T on creep behavior
![Page 3: CREEP TEST COMPLETE.pdf](https://reader035.fdocuments.us/reader035/viewer/2022072922/54619533b1af9f936c8b49b9/html5/thumbnails/3.jpg)
RESULTS
Specimens number Specimen 1 Load
87N
Specimen 2 Load
90 N
Specimen 3 Load
93 N
Load, m [kg] 8.869 kg 9.174 kg 9.48 kg
Specimen thickness, h
[mm] 0.17 mm 0.17 mm 0.17 mm
Specimen width of the
gauge length,
d [mm]
10.78 mm 10.78 mm 10.78 mm
Initial gauge length, l0
[mm] 10 mm 10 mm 10 mm
Final gauge length,
l [mm] 14.1 mm 14.1 mm 13.8 mm
Specimen 1 Load 87N
![Page 4: CREEP TEST COMPLETE.pdf](https://reader035.fdocuments.us/reader035/viewer/2022072922/54619533b1af9f936c8b49b9/html5/thumbnails/4.jpg)
Specimen 1 Load 90 N
time (s) elongation (mm) strain
5 1.5 0.15
10 1.6 0.16
15 1.65 0.165
20 1.7 0.17
25 1.75 0.175
30 1.8 0.18
35 2.83 0.283
40 1.85 0.185
45 1.9 0.19
50 1.95 0.195
55 1.97 0.197
60 1.99 0.199
65 2.1 0.21
70 2.3 0.23
75 2.5 0.25
79.2 4 0.4
time (s) elongation (mm) strain
5 1.3 0.13
10 1.4 0.14
15 1.6 0.16
20 1.8 0.18
22.8 4 0.4
![Page 5: CREEP TEST COMPLETE.pdf](https://reader035.fdocuments.us/reader035/viewer/2022072922/54619533b1af9f936c8b49b9/html5/thumbnails/5.jpg)
Specimen 1 Load 93 N
time (s) elongation (mm) strain
5 1.4 0.14
10 1.6 0.16
15 1.65 0.165
20 1.8 0.18
25 2.2 0.22
26.4 3.8 0.38
![Page 6: CREEP TEST COMPLETE.pdf](https://reader035.fdocuments.us/reader035/viewer/2022072922/54619533b1af9f936c8b49b9/html5/thumbnails/6.jpg)
Discussion
1. From the experiment result, how is the shape of obtained creep rate curves?
Figure 1: Creep curve graph for plastic
Following the loading strain εο, the creep rate (slope of strain vs time curve), is high but decreases
as the material deforms during the primary creep stage. At sufficiently large strains, the material creeps at
a constant rate. This is called the secondary or steady-state creep stage. Ordinarily this is the most
important stage of creep since the time to failure tf is determined primarily by the secondary creep rate. In
the case of tension creep, the secondary creep stage is eventually interrupted by the onset of tertiary
creep, which is characterized by internal fracturing of the material, creep acceleration,
and finally failure.
2. How is the results compared to the theory?
A typical creep curve for a plastic specimen is shown in Figure 1. The initial part of the characteristic shows the three stages of creep. The strain has been calculated by dividing the different in length (4.1mm) over original length (10mm), which gives an elastic strain of 0.41. For the theory calculation which is 669.6E (E=Modulus of elasticity), there might be a slight different from the result obtained from the experiment. The higher the load being applied to the specimen the faster the time taken for the specimen to reach fracture period. However, this result is for a higher stress and very much shorter creep time than would normally be used for material testing
![Page 7: CREEP TEST COMPLETE.pdf](https://reader035.fdocuments.us/reader035/viewer/2022072922/54619533b1af9f936c8b49b9/html5/thumbnails/7.jpg)
3. How do you summarize the occurred errors, and discuss the factors affected to the
experimental results?
One of the error occurred when doing the experiment is that the size measure and
the real size of the specimen is not precise, thus making the error happen. Another factor
that most likely to cause the experiment to has an error from the theory result is that the
specimen is not carefully cut from its required shape. It make the specimen have a small
unnecessary cut that make the specimen comes to fracture stage faster than usual.
Moreover, temperature of the surrounding also affects the experimental result. This is
because at high temperatures the entire creep process can occur in a matter of seconds. The last error that
might occurred is the apparatus or equipment used showed error before the experiment or the placing of
the specimen onto the universal testing machine is not correct or slightly misplace.
Conclusion
As a conclusion, we know that the creep test is conducted using a tensile specimen which
a constant stress is applied, often by the simple method of suspending weights from it.
Deformation is recorded at specified time intervals and a creep vs. time diagram is plotted. Slope
of curve at any point is creep rate. If failure occurs, it terminates test and time for rupture is
recorded. If specimen does not fracture within test period, creep recovery may be
measured. Creep is generally divided into three stages. The primary creep starts at a rapid rate
and slows with time. The secondary creep has a relatively uniform rate and the tertiary creep has
an accelerated creep rate and terminates when the material breaks or ruptures. If creep recovery
is measured, the test will determine the stress-relaxation. The rate of decrease in deformation that
takes place when the load is removed. Creep is also sometimes referred to as Stress-Relaxation
testing.
Reference
Hashemi, S. Foundations of materials science and engineering, 2006, 4th edition,
McGraw Hill, ISBN 007-125690-3
Dieter, G.E., Mechanical metallurgy, 1988, SI metric edition, McGraw-Hill, ISBN 0-07-
100406-8.
![Page 8: CREEP TEST COMPLETE.pdf](https://reader035.fdocuments.us/reader035/viewer/2022072922/54619533b1af9f936c8b49b9/html5/thumbnails/8.jpg)