BRE Global Test Report - Morland · BRE Global Ltd Watford, Herts WD25 9XX Customer Services 0333...

9
BRE Global Test Report BS 476-6: 1989 + A1: 2009 Fire propagation test on Vinyl faced Plaster board (MOR103437, Plasterboard White Linen 1/S) Prepared for: Morland Date: 22 October 2019 Report Number: Q100931-1003 Issue 1 BRE Global Ltd Watford, Herts WD25 9XX Customer Services 0333 321 8811 From outside the UK: T + 44 (0) 1923 664000 F + 44 (0) 1923 664010 E [email protected] www.bre.co.uk Prepared for: Morland Unit 4, Buttington Cross Enterprise Park, Welshpool, Powys, SY21 8SL

Transcript of BRE Global Test Report - Morland · BRE Global Ltd Watford, Herts WD25 9XX Customer Services 0333...

BRE Global Test Report BS 476-6: 1989 + A1: 2009 Fire propagation test on Vinyl faced

Plaster board (MOR103437, Plasterboard White Linen 1/S)

Prepared for: Morland

Date: 22 October 2019

Report Number: Q100931-1003 Issue 1

BRE Global Ltd Watford, Herts WD25 9XX Customer Services 0333 321 8811 From outside the UK: T + 44 (0) 1923 664000 F + 44 (0) 1923 664010 E [email protected] www.bre.co.uk

Prepared for: Morland Unit 4, Buttington Cross Enterprise Park, Welshpool, Powys, SY21 8SL

Fire propagation test to BS 476-6: 1989 + A1: 2009 Report Number: Q100931-1003: Issue 1

Commercial in Confidence © BRE Global Ltd 2019

Page 1 of 8

This report is made on behalf of BRE Global and may only be distributed in its entirety, without amendment, and with attribution to BRE Global Ltd to the extent permitted by the terms and conditions of the contract. Test results relate only to the specimens tested. BRE Global has no responsibility for the design, materials, workmanship or performance of the product or specimens tested. This report does not constitute an approval, certification or endorsement of the product tested and no such claims should be made on websites, marketing materials, etc. Any reference to the results contained in this report should be accompanied by a copy of the full report, or a link to a copy of the full report.

BRE Global’s liability in respect of this report and reliance thereupon shall be as per the terms and conditions of contract with the client and BRE Global shall have no liability to third parties to the extent permitted in law.

Opinions and interpretations expressed herein are outside the scope of UKAS Accreditation.

Prepared by

Name B Gohil

Position Technician

Signature

Authorised by

Name M Walford

Position Chemist

Date 22 October 2019

Signature

Fire propagation test to BS 476-6: 1989 + A1: 2009 Report Number: Q100931-1003: Issue 1

Commercial in Confidence © BRE Global Ltd 2019

Page 2 of 8

Table of Contents

1 Objective 3 2 Sample 3

2.1 Traceability 3

2.2 Description of sample and test format. 3

3 Conditioning 4 4 Results 4

4.1 Temperature measurement 4

4.2 Observations 5

5 Conclusions 5 6 Validity 5 7 Reference 5 Appendix A Product description provided by the test sponsor 6 Appendix B Sample photographs 7

Fire propagation test to BS 476-6: 1989 + A1: 2009 Report Number: Q100931-1003: Issue 1

Commercial in Confidence © BRE Global Ltd 2019

Page 3 of 8

1 Objective

To determine the fire propagation index of the sample specified in Section 2 using the test method specified in British Standard 476: Part 6: 1989 + A1: 20091.

2 Sample

2.1 Traceability The test samples were supplied by the test sponsor. BRE Global were not involved in the sample selection process and therefore cannot comment upon the relationship between the samples supplied for test and the product supplied to market.

2.2 Description of sample and test format. Unless otherwise stated all measurements are nominal.

Test Sponsor Morland. Unit 4, Buttington Cross Enterprise Park, Welshpool, Powys, SY21 8SL

Manufacturer of sample As Above

Sample name/reference MOR103437, Plasterboard White Linen 1/S.

Sample description (as provided by test sponsor/manufacturer)

Vinyl faced Plaster board (MOR103437, White Linen). White Linen (Dolomite) 46721 MDX304698 on Plasterboard 243643 MTX102164.

Full product description of the sample provided by the test sponsor is given in Appendix A.

Description of sample (as received by BRE Global)

White fabric like material slightly textured (approximately 0.3 mm thick) on plasterboard (approximately 9.2 mm thick).

Photographs of the sample are given in Appendix B.

Mean weight per unit area (kg/m2)

6.20

Mean thickness (mm) 9.52

Sample receipt date 30 August 2019 (BRE Ref E12241)

Test face White face

Test format With air gap

Date of test 04 October 2019

Purchase order number MP0606 Robin Hawkins

Fire propagation test to BS 476-6: 1989 + A1: 2009 Report Number: Q100931-1003: Issue 1

Commercial in Confidence © BRE Global Ltd 2019

Page 4 of 8

3 Conditioning

The specimens were conditioned as required by the standard.

4 Results

4.1 Temperature measurement Table 1 shows the Temperature rise for calibration sheet and specimens

Table 2 shows the Index of performance for each specimen

Table 1 – temperature rise

Time Temperature rise - °C

t Calibration Specimens min sheet a b c 0.5 13.4 17.3 18.2 17.0 1 19.6 24.0 26.0 25.5

1.5 24.1 29.6 32.3 32.0 2 28.1 34.3 35.6 34.5

2.5 31.2 37.0 38.1 37.5 3 33.8 39.8 40.9 39.6 4 66.3 70.4 71.2 72.1 5 104.9 110.7 109.6 111.2 6 130.0 141.0 137.7 139.1 7 151.9 161.9 162.2 159.5 8 166.9 181.0 179.6 178.9 9 180.2 194.3 195.0 196.8 10 190.2 201.7 205.3 209.2

12 203.2 221.8 219.8 227.6 14 215.7 230.3 237.3 236.2 16 223.0 239.9 247.3 244.4 18 228.0 247.3 252.2 250.4 20 234.8 249.3 255.3 254.8

t - time in minutes from the time at which the gas jets were ignited.

a, b and c - represent individual specimens giving valid test results.

Fire propagation test to BS 476-6: 1989 + A1: 2009 Report Number: Q100931-1003: Issue 1

Commercial in Confidence © BRE Global Ltd 2019

Page 5 of 8

Table 2 Index of performance

Specimen S s1 s2 s3

a 3.8 2.3 1.0 0.5 b 4.7 3.0 1.0 0.7 c 4.4 2.6 1.1 0.7

4.2 Observations No intumescence or deformation of any specimen occurred that affected the required gas input.

No melting or slumping occurred that prevented the material from being exposed to the heating conditions.

Air flow through the apparatus was not restricted by fallen material or by soot accumulation in the chimney.

5 Conclusions

A sample as described in this report, when tested in accordance with BS 476: Part 6: 1989 + A1: 2009, achieved: fire propagation index I = 4.2 sub-indices i1 = 2.6

i2 = 1.0

i3 = 0.6

BS 476: Part 6: 1989 + A1: 2009 does not contain acceptance criteria and therefore this test report does not indicate a pass or fail of the product.

6 Validity

The test results relate only to behaviour of the test specimens of the product under the particular conditions of test, they are not intended to be the sole criteria for assessing the potential fire hazard of the product in use.

7 Reference

1 British Standard 476: Part 6: 1989 + A1: 2009 Fire tests on building materials and structures. Part 6. Incorporating Corrigendum No 1:2014. Fire propagation test for products. British Standards Institution, London 2009.

Fire propagation test to BS 476-6: 1989 + A1: 2009 Report Number: Q100931-1003: Issue 1

Commercial in Confidence © BRE Global Ltd 2019

Page 6 of 8

Appendix A Product description provided by the test sponsor

Test sponsor: Unit 4, Buttington Cross Enterprise Park, Welshpool, Powys, SY21 8SL

Parameter Details (if applicable) Trade name vinyl faced Plaster board General description Plasterboard White Linen 1/S Name and address of manufacturer of product As above Place of manufacture As above Product reference/number MOR103437 Thickness 9.5mm Density 800kg/m3 Mass per unit area 7.6kgm2 Generic type of product Note 1 Flame retardant treatment added or organic content limited during production (yes/no), if yes give details

No

Harmonised EN product standard, and AVCP System No. if applicable

BS476-6 & 7 (Class 0)

Interior facing 1 - Generic type (test face) - Product reference - Manufacturer - Thickness - Mass per unit area/ density - Colour reference - Trade name flame retardant - Generic type flame retardant - Amount flame retardant

Vinyl Decor - White Linen (Dolomite) 46721 MDX304698 Note 1 100um Note 1 White None N/A N/A

Adhesive - Generic type (if applicable) - Product reference - Manufacturer - Application rate - Application method - Specific gravity - Colour reference - Trade name flame retardant - Generic type flame retardant - Amount flame retardant

Glue - Advatac RD9000 RD9000 Advatac 80 gsm Machine laminated Note 1 Note 1 None N/A N/A

Substrate - Generic type (if applicable) - Product standard - Product name/reference - Manufacturer - Thickness - Density or mass per unit area - Class (EN 13501-1)

MTX102164 Plasterboard 243643 MTX102164 Note 1 Note 1 Note 1 Note 1

Face to be tested Face Laminated with Paper backed vinyl Orientation aspects Note 1 Sampling Identification Reference Note 1 Additional information: Note 1

Note 1: This information was not provided by the test sponsor.

Fire propagation test to BS 476-6: 1989 + A1: 2009 Report Number: Q100931-1003: Issue 1

Commercial in Confidence © BRE Global Ltd 2019

Page 7 of 8

Appendix B Sample photographs

Front (Test face)

Side

Fire propagation test to BS 476-6: 1989 + A1: 2009 Report Number: Q100931-1003: Issue 1

Commercial in Confidence © BRE Global Ltd 2019

Report Ends

Page 8 of 8

Back