Batch and Roll-to-Roll Atomic Layer Deposition (ALD)
processing for ultra-barrier and other applications.
© 2014 Centre for Process Innovation Limited. All Rights Reserved.
ALF SMITH
![Page 2: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/2.jpg)
Who are CPI?
CPI is a UK technology innovation centre and the process element of the Government’s
High Value Manufacturing Catapult.
We use applied knowledge in science and engineering combined with state of the art
facilities to enable our clients to develop, prove, prototype and scale-up the next
generation of products and processes.
Sustainable Processing Centre
Thermal Technologies Centre
National Printable Electronics Centre
National Biologics Manufacturing Centre
![Page 3: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/3.jpg)
CPI - Printable Electronics OverviewCPI Printable Electronics is a design, development and prototyping facility for the emerging Printable Electronics (PE) industry.
Funded by :-
� ~33% Catapult (TSB, UK Government)
� ~33% Collaborative Development (UK, EU)
� ~33% Commercial Development (Global)
• Fabrication• Prototyping• Prototyping• Access to Scale-able Toolsets• Commercialisation Support• Incubator Space
Facilities– 2 clean rooms (Class100 &1000)– Formulation, optical, & electrical test labs– 12 incubator offices– Expert techno-commercial team
![Page 4: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/4.jpg)
WHY TRANSPARENT FLEXIBLE ULTRA-BARRIER?
![Page 5: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/5.jpg)
RIGID
ENCAPSULATION
FLEXIBLE
ENCAPSULATIONREPLACE GLASS
with
ULTRA-BARRIER POLYMER FILM
BENEFITS
• FLEXIBLE
• ROBUST
• LIGHTWEIGHT
• THIN
• TRANSPARENCY• TRANSPARENCY
ENABLES
• NEW PRODUCT DESIGN
- COMFORMABLE
- FLEXIBLE
• R2R LOW COST MANUFACTURING
- COATING
- LAMINATING
![Page 6: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/6.jpg)
PRINTABLE ELECTRONICS MARKET
22% ($1.3B) FLEXIBLE 43% ($23B) FLEXIBLE
PV
IDTechEx,2012
OLED
DISPLAY
OLED
LIGHT
![Page 7: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/7.jpg)
![Page 8: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/8.jpg)
Insufficient moisture barrier on OLED devices- electrode degradation
- causes dark spots
[Galand, 2010], effect of moisture ingress on
OLED device performance. Black spots are
caused by oxidation of the cathode
![Page 9: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/9.jpg)
WHAT IS TRANSPARENT FLEXIBLE ULTRA-BARRIER?
![Page 10: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/10.jpg)
Barrier layer requirements on plastic substrates
Water vapour barrier
g.m2.day-1
Polymer films 1s-100s
Food packaging 0.1-10Food packaging 0.1-10
Electro-Chromics 0.001-0.05
Flexible PV 0.00001-0.001
Flexible OLEDs 0.0000001-0.00001
![Page 11: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/11.jpg)
Application Moisture Barrier
g H2O/m2/day
Lifetime UV damage Flexibility Cost/m2
OLED Display 1 x 10-6 +5 -10 yrs X X � High
OLED SSL 1 x 10-6 +10-15 yrs X X � Med
OPV 1 x 10-3 -1 x 10-5 +25 Yrs � � Low
Ultra-Barrier layer requirements on plastic substrates
OPV 1 x 10-3 -1 x 10-5 +25 Yrs � � Low
Inorganic PV 1 x 10-2 - 1x 10-4 +25 Yrs � � Low
Barrier retention over product lifetime!
![Page 12: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/12.jpg)
Water Vapour Transmission Process
Solution and Diffusion
through coating and
substrate
Debris on
Grain boundaries
in coatings – not
for amorphous
layers
Delamination
of coating
Pinholes in
coating or
substrate
Defects in
125um PET
Debris on
surface of coating
? -100 nm barrier
Defects in
substrate
![Page 13: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/13.jpg)
Routes to Ultra-Barrier
1. Single layer – low defect density – near ‘perfect’
2. Multilayer (‘Vitex’ - type)
3. Multi-laminate structures
![Page 14: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/14.jpg)
![Page 15: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/15.jpg)
Single and multi-layer barriers
Barrier
• A key enabling technology for flexible electronics on plastic
Barrier layer
Inter-layer
Single ‘perfect’ layer
Plastic film Plastic filmSingle layer Multi-layer• Can be the substrate and encapsulation (packaging) for devices
• ‘Perfect’ layer can provide high barrier (high density, low defects)
• Multi-layer approach (e.g. Vitex)
Single ‘perfect’ layer
![Page 16: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/16.jpg)
Water vapour transmission through barriers of equivalent
total thickness
Time
H2O
(g/m2/day)
Low barrierMedium barrier
High barrier
Single barrier
Polymer
Lag times
Time
TimeDouble barrier
• follows R.Ash et al,
Brit.J.Appl.Phys. 1965
• see also G. Graff et al, J.Appl. Phys.
2004
H2O
(g/m2/day)
Assumption materials dry from the outset
![Page 17: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/17.jpg)
Multi-layer Barrier
• Deposition of thin (20 -
50nm) layers of inorganic
materials combined with
some organic polymeric thin
layerslayers
– Blocks porosity in polymer thin
films
– Dislocates pores providing
tortuous path
Barix Multilayers: a Water and Oxygen Barrier
for Flexible Organic Electronics
– Visser RJ: Vitex Systems. Nanoforum
![Page 18: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/18.jpg)
HELIATEK – small molecule evaporated OPV with Multi-layer barrier
ALUMINIUM
ORGANIC
ITOPOLYMERINORGANIC
BARRIER
200nm
POLYMER
POLYMER
POLYMER
INORGANIC
INORGANIC
INORGANIC
![Page 19: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/19.jpg)
Multi-layer; ‘VITEX’ Approach
• Multi-inorganic barrier/organic interlayers (multi-DIAD)
• Several players (e.g. 3M, Samsung)• Several players (e.g. 3M, Samsung)
• Cost?
• Robustness in original form?
![Page 20: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/20.jpg)
POLO ULTRA-BARRIER
Fraunhofer (IVV, FEP, ISC)
![Page 21: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/21.jpg)
Multi-layer/Nanoparticle -Tera Barrier Films, Singapore
![Page 22: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/22.jpg)
GE GRADED ULTRA-BARRIER
low 10-5~mid 10-6 g/m2/day(at 23°C 50 % RH)low 10-5~mid 10-6 g/m2/day(at 23°C 50 % RH)
![Page 23: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/23.jpg)
APPLIED MATERIALS
• Barrier with single layer PECVD SiNx silane-based
process.
• R2R production
• ~5x 10-5 g/m2/day @ 20C/50%RH by Ca Test
(300nm on PEN).
• Developing Organic polymer/SiNx diad multi-layer
structures•
structures
~4x10-3g/m2/day
![Page 24: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/24.jpg)
HOLST CENTRE, EINDHOVEN
Barrier Technology:PECVD SiN/ORGANIC LAYER/PECVD SiN
• DIRECT ENCAPSULATION ON OLED DEVICE
• DAMP HEAT TEST 500hrs, 60C/90%RH, 97% yield for no black
spots
• Applying to R2R, Applying to barrier film.• Applying to R2R, Applying to barrier film.
“We have successfully produced over 2.5 kilometers of
R2R barrier film based on a single inorganic layer with
water vapour transmission rates (WVTR) lower than
10-5 g/m2 per day on commercial-grade PET foil,”
Microwave plasma sources
![Page 25: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/25.jpg)
AEGIS Deposition System
1.4m wide R2R
500,000m2/year
~1-2m/min
~1x10-5 g/m2/day 23C/50% RH
![Page 26: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/26.jpg)
FLEXIBLE GLASS CORNING
COST!
• Stability
• R2R compatible
• Smoothness
• Outstanding barrier performance
ROBUSTNESS!COST!ROBUSTNESS!
![Page 27: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/27.jpg)
Transparent Ultra-Barrier by
CPI’s IMMEDIATE INTEREST:
Transparent Ultra-Barrier by
Atomic Layer Deposition (ALD)
![Page 28: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/28.jpg)
Batch ALD: Al2O3 using TMA and H2O
• Two chemical precursors react in a type of cyclical CVD process
• Reaction is self-limiting and stops at the end of each cycle
• For Al2O3 deposition the precursors are typically:
– Trimethyl-aluminium (TMA)
– H2O or O2 plasma or ozone for oxidation (CPI has all available)– H2O or O2 plasma or ozone for oxidation (CPI has all available)
• The 4 steps below constitute 1 cycle for Al2O3 using TMA + H2O
1.TMA chemisorption 2. TMA purge 3. H2O exposure 4. H2O & CH4 purge
![Page 29: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/29.jpg)
Properties of ALD coatingsBecause ALD is a surface-mediated gas phase process the films have the following characteristics:
– Highly-conformal – uniform coatings into high aspect-ratio trenches, over step edges and into complex 3D objects
– Low stress – good adhesion; important for MEMS and sensors
– Dense, with few defects – relatively free of pinholes as required for barriers and – Dense, with few defects – relatively free of pinholes as required for barriers and encapsulation
– Reproducible – ‘digital’ thickness control on sub-nm scale
– Different materials can be combined to form nano-scale laminates
– Deposition can be done at low temperature (even at RT)
– Deposition rates are typically ~0.5-1.5nm/min (process specific)
– Amorphous or partially crystalline films (process specific)
![Page 30: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/30.jpg)
ALD coating of high aspect-ratio features [GENUS]
Highly conformal multilayer films
High-k Dielectrics for DRAM Capacitors
![Page 31: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/31.jpg)
Oxford Instruments
• FlexALTM tool designed for processing
semiconductor wafers
• Batch process: coating up to max 200mm wafer
140mm x 140mm
Atomic Layer Deposition (ALD) Batch Coaters
Beneq TFS500
• various internal process chambers
• coating to 370x470mm (GEN 2 size)
• Thermal and plasma (capacitive, to 300mm dia.)
![Page 32: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/32.jpg)
Batch ALD samples produced on polymer films:
• Extrinsic barrier (large area measurement)
MOCON Aquatran 1: < 5x10-4 g/m2/day
• Intrinsic barrier (small area)
Laser spot Ca Test: ~1-2 x 10-6 g/m2/dayLaser spot Ca Test: ~1-2 x 10 g/m /day
Excellent reproducibility at AlOx thickness >20nm
![Page 33: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/33.jpg)
Mocon measurements on ALD barriers
1.5
2
2.5
3
3.5W
VT
R (
10
^-3
g/m
^2
/da
y)
40nm (20 samples)
20nm (2 samples)
10nm (2 samples)
Batch ALD planarised PEN substrate
0
0.5
1
1.5
0 10 20 30 40 50
Barrier thickness (nm)
WV
TR
(1
0^
-3 g
/m^
2/d
ay
)
10nm (2 samples)
5 nm (2 samples)
• Barrier possible at <10nm thicknesses in batch• 15nm thick barrier realised in R2R, <5x10-4 g/m2/day @ 0.4m/min
Detection LimitAquatran 1
![Page 34: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/34.jpg)
1.E-03
1.E-02
WV
TR
[g
/m2/d
ay]
Mocon:
Sample 10 x10 cm2: measured area 50cm2
1.E-04
12D
2701 (F
)
12D
2702 (B
)
12D
2703 (F
)
12D
2704 (B
)
12D
2705 (F
)
12D
2706 (B
)
12D
3001 (F
)
12D
3001 (B
)
12F
0601
12F
0602
12F
0603
12F
0604
12F
0605
12F
0606
12F
0607
12F
0608
Sequence of samples
WV
TR
[g
/m2/d
ay]
Mocon: lower sensitivity limit
Early barrier samples
With better handling and chamber conditioning
![Page 35: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/35.jpg)
• high barrier performance with no lag time
• intrinsic WVTR @ ~1x10-6 g/m2/day
• amorphous high density barrier layers
Barrier layer benefits of ALD
• amorphous high density barrier layers
• low materials usage and costs
• key issue is to overcome defects (particles)
![Page 36: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/36.jpg)
Best values:
2 x 10-5 g/m2/day
@ 26C, 80%RH
Single ALD layer,
Batch production
CALIBRATED Ring-down laser absorption
Lowest detectivity
2 x 10-5 g/m2/day
76cm2 sample area
4 x 10 -5g/m2/day
@ 35C, 90%RH
![Page 37: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/37.jpg)
0.60
0.80
1.00
1.20
rel.
Eta Epoxy-ALD-Epoxy
Epoxy-ALD-Epoxy
DH degradation of monolithically integrated CIGS submodules
on glass substrates (10x10 cm2) - ~15% eff.
0.00
0.20
0.40
0.60
V LS 100h DH 295h DH 633h DH 1040h DH LS2 2044h DH LS3
rel.
Eta
Epoxy-ALD-Epoxy
Epoxy-ALD-Epoxy
1000 h 2000 h
DH 80C, 80%RHLS = Light soak recovery
![Page 38: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/38.jpg)
0.40
0.50
0.60
0.70
0.80
0.90
1.00
1.10
rel.
eta
310h DH 1000h DH and LS
DH degradation of monolithically integrated CIGS submodules on glass substrates
(10x10 cm2) - ~15% eff.
0.00
0.10
0.20
0.30
0.40
Encapsulations (E=Epoxy; ALD= AlOx)
![Page 39: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/39.jpg)
R2R ALD – Spatial ALD
![Page 40: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/40.jpg)
R2R Spatial ALDExamples
-Levitech
- Solay Tech
- Beneq
- TNO/VDL Flow
++++
Example: TNO
Homogeneous
deposition of Al2O3 :
layer thickness of ~23
nm at 0.5 m/min web
speed and 0.5 Hz drum
rotation
REVEIW PAPER:
P. Poodt. D. Cameron, E. Dickey, S.M. George, V. Kuznetsov,
G.N. Parsons, F. Roozeboom, G. Sundaram, A. Vermeer, JVST-
A 30 (2012) 10802
![Page 41: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/41.jpg)
LOTUS APPLIED TECHNOLOGY
Serpentine web translation, single-sided coating
300 mm wide web, up to 600 meters long
25 roller pairs: up to 100 ALD cycles in a single-pass
Suitable for web widths < 1.5 meters and thickness > 100
μm
Produced 6 nm barrier film @ 30 m/min with WVTR < 5 x
10-4 g/(m2·d)
COIL REACTOR – concept only
Single-sided web contact only: well-suited for
widths > 1.5 m, thickness < 100 μm
Each lap = 4 complete ALD cycles
7 laps @ 300 m/min ~5 nm ALD film thickness
~0.005 g/(m2·d) WVTR
Cost estimate $0.03/m2
![Page 42: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/42.jpg)
• Excellent prospects to scaling to +1 meter widths, due to reasonable mechnical tolerances
– 0.5 mm gap across 500 mm web width
• Second generation systems built.
Collaboration between hardware and process development companies.
• Collaboration with the Centre for Process Innovation (UK)
– Facilitates rapid technology engagement with industry
– CPI will collaborate with institutes and companies Globally for wide range application for R2R ALD.
• Roadmap for R2R ALD
– Scaling beyond 500 mm, line-integration
– Further web speed improvement by PEALD
– Pre-and post-processes to address particles
Now Operational at CPI
![Page 43: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/43.jpg)
Key focus for R2R ALD development:
• production line speeds of >1 m/min
• small machine footprint
web width 0.5m
CPI R2R ALD development
• web width 0.5m
• thin high density barrier layers
• methods to reduce defects + effect of defects
• robust mechanical barrier materials
• low production cost
![Page 44: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/44.jpg)
CPI R2R ALD system. Coating System 600 & Side pod
![Page 45: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/45.jpg)
13/11/2015
![Page 46: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/46.jpg)
R2R ALD deposition.
• TMA + Water process
• Substrate metallised PET
![Page 47: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/47.jpg)
• Process tuning phase
• Short rolls of barrier produced
• Early stage barrier performance promising
15 – 40nm thick AlOx on 125 micron thick PET+PEN has shown
R2R-ALD PROCESS PERFORMANCE
15 – 40nm thick AlOx on 125 micron thick PET+PEN has shown
extrinsic barrier:
< 5 x 10-4 g/m2/day (Mocon Aquatran 1)
• Shown at 0.1, 0.2 and 0.4 m/min (40, 20, 15nm thick)
• Substrate temperature 105°C
• Extensive measurements underway
![Page 48: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/48.jpg)
R2R ALD barrier demonstration
• Coated using WCS 500 (R2R ALD pilot).....operated at LUT Univ. Finland
• Substrate is Dupont Teijin OPTIFINE PEN (125 µm)
• 20 nm thick Al2O3, from TMA + H2O
• Process temperature 105 C
• Coating width 500 mm, samples cut out to 120 x 120 mm
![Page 49: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/49.jpg)
Optical calcium test device200 mm
• Characaterization courtersy to L. Moro & Z. Zeng (S. Cheil Industries)
• Temporary barrier is not good barrier under 85 C / 85 % relative humidity conditions
• Barrier foil sample not large eneough to cover full Ca test device area -> permation from
sides taking place, only A and B areas considered for WVTR
J. Vac. Sci. Technol. A 32(5) Sep/Oct2014
![Page 50: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/50.jpg)
Ca test results
A
B
• No clear pin-hole generation or growth observed
• WVTR ~5.0E-6 g/m2/day at 20C/50%RH is estimated
• Ca test stopped after 800hrs at 85C/85%RH due to edge penetration, but the barrier itself is still good
• Samples also measured with MOCON Aquatran 1, repeated measurements
<5*10-4 g/(m2 day) at 40 C / 90 % RH
a) 185 hours at 40 C / 90 % rh
b) 468 hours at 85 C / 85 % rh
c) 800 hours at 85 C / 85 % rh
![Page 51: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/51.jpg)
FUTUREUltra-barrier Targets
• Line speed >5m/min
• Barrier 1 x 10-6 g/m2/day
• Barrier coating cost <$10/m2
Other coatings
• as direct encapsulation (OLED, PV, PE, SENSORS)
• as Nano-laminates (new materials)
• as ‘perfect’ interfaces
• as Contacts (work function control)
• as Gate dielectrics
• TFT devices
• PV structures
• Surface active coatings.
• Smart Coatings
![Page 52: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/52.jpg)
R2R -CIGS
CPI member of FP7 large project R2R-CIGSPartners:
TNO (NL), EMPA (CH), FLISOM (CH), ZSW (DE), ISOVOLTAIC (AU), MANZ (DE), TNO (NL), EMPA (CH), FLISOM (CH), ZSW (DE), ISOVOLTAIC (AU), MANZ (DE),
BENEQ (FI), SOLAY-TEC (NL), MONDRAGON (ES)
Full R2R pilot production line for flexible CIGS solar cells
Clear Barrier Foil for thin film CIGS flexible PV
Direct encapsulation of thin film CIGS flexible PV
![Page 53: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/53.jpg)
15 partners, European Framework 7 Programme– NMP-2011 NanoSciencies, NanoTechnologies, Materials and New Production Technologies.
EMFT
The NanoMend project has received funding from the European
Community’s Seventh Framework Program (FP7/2007-2013) UNDER
Grant Agreement No. 280581
![Page 54: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/54.jpg)
HIBPE – Innovate UK project
CPI, Sedgefield
CAMVAC Ltd., Thetford
G24 Power Ltd., NewportG24 Power Ltd., Newport
Inside 2 Outside Ltd. (I2O), Cambs
Tata Steel UK
SPECIFIC, Swansea
![Page 55: Batch and Roll-to-Roll Atomic Layer Deposition (ALD ... · PDF fileBatch and Roll-to-Roll Atomic Layer Deposition (ALD) processing for ultra-barrier and other applications. ... •](https://reader031.fdocuments.us/reader031/viewer/2022021421/5a8b49dc7f8b9a7f398c2932/html5/thumbnails/55.jpg)
Conclusion
1. Many promising Ultra-barrier technologies
2. ALD technology has high potential for Ultra-barrier applications
3. R2R ALD possible
4. Other applications for ALD and R2R ALD insight