Date: 3/30/2012 Authorized by: Abdul MuisChemist
Page 1 of 8
PT. Nalco IndonesiaAnalytical Resources
Jl.Pahlawan Desa Karang Asem Timur , Citeureup – Bogor 16810Phone ( 021) 875-3175, Fax (021) 875-3167.
Customer : PT. Cahaya Fajar Kaltim Sample Number : 215RSN12 (1)Date received : Mar. 22, 2012
Nalco Representative : Ariyanto Pangkung Date sampled : Feb. 16, 2012Date completed : Mar. 30, 2012
RESIN ANALYSIS REPORT
Sampel Marked : RESIN ANION A
TOTAL EXCHANGE CAPACITY (BEFORE CLEANING)
Milliequivalents/milliliter (wet) 0.76
TOTAL EXCHANGE CAPACITY (AFTER CLEANING)
Milliequivalents/milliliter (wet) 0.82
CONDITION OF RESIN
Physical Condition of Resin :
% Normal Beads 82
% Broken & Cracked Beads 18
Fouling HEAVY
RECCOMENDATION
Replace with new resin
-
8/18/2019 Analisa Resin CFK
2/8
Date: 3/30/2012 Authorized by: Abdul MuisChemist
Page 2 of 8
PT. Nalco IndonesiaAnalytical Resources
Jl.Pahlawan Desa Karang Asem Timur , Citeureup – Bogor 16810Phone ( 021) 875-3175, Fax (021) 875-3167.
Customer : PT. Cahaya Fajar Kaltim Sample Number : 215RSN12 (2)Date received : Mar. 22, 2012
Nalco Representative : Ariyanto Pangkung Date sampled : Feb. 16, 2012Date completed : Mar. 30, 2012
RESIN ANALYSIS REPORT
Sampel Marked : RESIN ANION B
TOTAL EXCHANGE CAPACITY (BEFORE CLEANING)
Milliequivalents/milliliter (wet) 0.74
TOTAL EXCHANGE CAPACITY (AFTER CLEANING)
Milliequivalents/milliliter (wet) 0.81
CONDITION OF RESIN
Physical Condition of Resin :
% Normal Beads 81
% Broken & Cracked Beads 19
Fouling HEAVY
RECCOMENDATION
Replace with new resin
-
8/18/2019 Analisa Resin CFK
3/8
Date: 3/30/2012 Authorized by: Abdul MuisChemist
Page 3 of 8
PT. Nalco IndonesiaAnalytical Resources
Jl.Pahlawan Desa Karang Asem Timur , Citeureup – Bogor 16810Phone ( 021) 875-3175, Fax (021) 875-3167.
Customer : PT. Cahaya Fajar Kaltim Sample Number : 215RSN12 (3)Date received : Mar. 22, 2012
Nalco Representative : Ariyanto Pangkung Date sampled : Feb. 16, 2012Date completed : Mar. 30, 2012
RESIN ANALYSIS REPORT
Sampel Marked : RESIN ANION MIXED BED A
TOTAL EXCHANGE CAPACITY (BEFORE CLEANING)
Milliequivalents/milliliter (wet) 0.84
TOTAL EXCHANGE CAPACITY (AFTER CLEANING)
Milliequivalents/milliliter (wet) 0.98
CONDITION OF RESIN
Physical Condition of Resin :
% Normal Beads 97
% Broken & Cracked Beads 3
Fouling MODERATE
RECCOMENDATION
Clean Resin with Resin Cleaner Chemical
-
8/18/2019 Analisa Resin CFK
4/8
Date: 3/30/2012 Authorized by: Abdul MuisChemist
Page 4 of 8
PT. Nalco IndonesiaAnalytical Resources
Jl.Pahlawan Desa Karang Asem Timur , Citeureup – Bogor 16810Phone ( 021) 875-3175, Fax (021) 875-3167.
Customer : PT. Cahaya Fajar Kaltim Sample Number : 215RSN12 (4)Date received : Mar. 22, 2012
Nalco Representative : Ariyanto Pangkung Date sampled : Feb. 16, 2012Date completed : Mar. 30, 2012
RESIN ANALYSIS REPORT
Sampel Marked : RESIN ANION MIXED BED B
TOTAL EXCHANGE CAPACITY (BEFORE CLEANING)
Milliequivalents/milliliter (wet) 0.84
TOTAL EXCHANGE CAPACITY (AFTER CLEANING)
Milliequivalents/milliliter (wet) 0.98
CONDITION OF RESIN
Physical Condition of Resin :
% Normal Beads 97
% Broken & Cracked Beads 3
Fouling MODERATE
RECCOMENDATION
Clean Resin with Resin Cleaner Chemical.
-
8/18/2019 Analisa Resin CFK
5/8
-
8/18/2019 Analisa Resin CFK
6/8
Date: 3/30/2012 Authorized by: Abdul MuisChemist
Page 6 of 8
PT. Nalco IndonesiaAnalytical Resources
Jl.Pahlawan Desa Karang Asem Timur , Citeureup – Bogor 16810Phone ( 021) 875-3175, Fax (021) 875-3167.
Customer : PT. Cahaya Fajar Kaltim Sample Number : 215RSN12 (6)Date received : Mar. 22, 2012
Nalco Representative : Ariyanto Pangkung Date sampled : Feb. 16, 2012Date completed : Mar. 30, 2012
RESIN ANALYSIS REPORT
Sampel Marked : RESIN KATION B
TOTAL EXCHANGE CAPACITY (BEFORE CLEANING)
Milliequivalents/milliliter (wet) 1.76
TOTAL EXCHANGE CAPACITY (AFTER CLEANING)
Milliequivalents/milliliter (wet) 1.92
CONDITION OF RESIN
Physical Condition of Resin :
% Normal Beads 98
% Broken & Cracked Beads 2
Fouling MODERATE
RECCOMENDATION
Clean Resin with Resin Cleaner Chemical.
-
8/18/2019 Analisa Resin CFK
7/8
Date: 3/30/2012 Authorized by: Abdul MuisChemist
Page 7 of 8
PT. Nalco IndonesiaAnalytical Resources
Jl.Pahlawan Desa Karang Asem Timur , Citeureup – Bogor 16810Phone ( 021) 875-3175, Fax (021) 875-3167.
Customer : PT. Cahaya Fajar Kaltim Sample Number : 215RSN12 (7)Date received : Mar. 22, 2012
Nalco Representative : Ariyanto Pangkung Date sampled : Feb. 16, 2012Date completed : Mar. 30, 2012
RESIN ANALYSIS REPORT
Sampel Marked : RESIN KATION MIXED BED A
TOTAL EXCHANGE CAPACITY (BEFORE CLEANING)
Milliequivalents/milliliter (wet) 1.78
TOTAL EXCHANGE CAPACITY (AFTER CLEANING)
Milliequivalents/milliliter (wet) 1.95
CONDITION OF RESIN
Physical Condition of Resin :
% Normal Beads 98
% Broken & Cracked Beads 2
Fouling MODERATE
RECCOMENDATION
Clean Resin with Resin Cleaner Chemical.
-
8/18/2019 Analisa Resin CFK
8/8
Date: 3/30/2012 Authorized by: Abdul MuisChemist
Page 8 of 8
PT. Nalco IndonesiaAnalytical Resources
Jl.Pahlawan Desa Karang Asem Timur , Citeureup – Bogor 16810Phone ( 021) 875-3175, Fax (021) 875-3167.
Customer : PT. Cahaya Fajar Kaltim Sample Number : 215RSN12 (8)Date received : Mar. 22, 2012
Nalco Representative : Ariyanto Pangkung Date sampled : Feb. 16, 2012Date completed : Mar. 30, 2012
RESIN ANALYSIS REPORT
Sampel Marked : RESIN KATION MIXED B
TOTAL EXCHANGE CAPACITY (BEFORE CLEANING)
Milliequivalents/milliliter (wet) 1.71
TOTAL EXCHANGE CAPACITY (AFTER CLEANING)
Milliequivalents/milliliter (wet) 1.94
CONDITION OF RESIN
Physical Condition of Resin :
% Normal Beads 98
% Broken & Cracked Beads 2
Fouling MODERATE
RECCOMENDATION
Clean Resin with Resin Cleaner Chemical.