WELDING PROCEDURE SPECIFICATION No. EPI-11- WP6 Rev. 1

Post on 24-Dec-2021

5 views 0 download

Transcript of WELDING PROCEDURE SPECIFICATION No. EPI-11- WP6 Rev. 1

WELDING PROCEDURE SPECIFICATION No. EPI-11- WP6 Rev. 1 May 30, 2013 Company: Enbridge Pipelines Inc., PO Box 398, 10201 Jasper Avenue, Edmonton, AB T5J 2J9 Scope: This welding procedure specification details the procedure to be followed for Thru-Wall or

Partial Wall Repair Welding of pipe as required by CSA Standard Z662-11 Oil and Gas Pipeline Systems.

Service Restrictions: Sweet or Sour Temperature Restrictions: Notch Toughness Tested to -5°C (23°F)

1. WELDING PROCESS & METHOD

Shielded Metal Arc Welding (SMAW) - Manual Method

2. JOINT GEOMETRY

a) Joint Type: Groove – Single Vee Butt b) Bevel Angle: See Drawing c) Root Face: 1.6 mm (0.063 in.), ±0.8 mm (0.032 in.) d) Root Gap: 1.6 mm (0.063 in.), ±0.8 mm (0.032 in.)

The surfaces to be welded shall be smooth, uniform, free of fins, laminations, tears, scale, slag, grease, paint or other foreign matter, which may adversely affect the welding.

3. BASE MATERIAL

a) Composition: This specification applies to pipe and/or component material manufactured in accordance with, or listed as “Acceptable Alternative Materials” in any of the following standards:

CSA Z662, Oil and Gas Pipeline Systems CAN/CSA-Z245.1 Steel Line Pipe CAN/CSA-Z245.11, Steel Fittings CAN/CSA-Z245.12, Steel Flanges CAN/CSA-Z245.15, Steel Valves

b) Material Grades 483 MPa (SMYS) or less c) Wall Thickness Qualified: 4.0 to 19.875 mm (0.157 to 0.782 in.) inclusive d) Pipe Diameter Qualified: 381 mm (15 in.) OD minimum e) CSA Carbon Equivalent: 0.32 maximum for >Gr.386 (SMYS)

4. FILLER METAL CLASSIFICATION & SIZE

a) Root Pass: E6010; 4.0 mm (5/32 in.) b) Hot Pass: E8010-G; 4.0 mm or 5.0 mm (5/32 or 3/16 in.) c) Fill Pass (es): E8018-C3; 2.4, 3.2 or 4.0 mm (3/32, 1/8 or 5/32 in.) d) Cap Pass (es): E8018-C3; 2.4, 3.2 or 4.0 mm (3/32, 1/8 or 5/32 in.)

5. POSITION & DIRECTION OF WELDING

a) Position: 5G (Pipe Horizontal, Fixed Position) b) Direction of Welding: Vertical Down

WELDING PROCEDURE SPECIFICATION No. EPI-11- WP6 Rev. 1 May 30, 2013 Company: Enbridge Pipelines Inc., PO Box 398, 10201 Jasper Avenue, Edmonton, AB T5J 2J9 Scope: This welding procedure specification details the procedure to be followed for Thru-Wall or

Partial Wall Repair Welding of pipe as required by CSA Standard Z662-11 Oil and Gas Pipeline Systems.

Service Restrictions: Sweet or Sour Temperature Restrictions: Notch Toughness Tested to -5°C (23°F)

1. WELDING PROCESS & METHOD

Shielded Metal Arc Welding (SMAW) - Manual Method

2. JOINT GEOMETRY

a) Joint Type: Groove – Single Vee Butt b) Bevel Angle: See Drawing c) Root Face: 1.6 mm (0.063 in.), ±0.8 mm (0.032 in.) d) Root Gap: 1.6 mm (0.063 in.), ±0.8 mm (0.032 in.)

The surfaces to be welded shall be smooth, uniform, free of fins, laminations, tears, scale, slag, grease, paint or other foreign matter, which may adversely affect the welding.

3. BASE MATERIAL

a) Composition: This specification applies to pipe and/or component material manufactured in accordance with, or listed as “Acceptable Alternative Materials” in any of the following standards:

CSA Z662, Oil and Gas Pipeline Systems CAN/CSA-Z245.1 Steel Line Pipe CAN/CSA-Z245.11, Steel Fittings CAN/CSA-Z245.12, Steel Flanges CAN/CSA-Z245.15, Steel Valves

b) Material Grades 483 MPa (SMYS) or less c) Wall Thickness Qualified: 4.0 to 19.875 mm (0.157 to 0.782 in.) inclusive d) Pipe Diameter Qualified: 381 mm (15 in.) OD minimum e) CSA Carbon Equivalent: 0.27 maximum for >Gr.386 (SMYS)

4. FILLER METAL CLASSIFICATION & SIZE

a) Root Pass: E6010; 4.0 mm (5/32 in.) b) Hot Pass: E8010-G; 4.0 mm or 5.0 mm (5/32 or 3/16 in.) c) Fill Pass (es): E8018-C3; 2.4, 3.2 or 4.0 mm (3/32, 1/8 or 5/32 in.) d) Cap Pass (es): E8018-C3; 2.4, 3.2 or 4.0 mm (3/32, 1/8 or 5/32 in.)

5. POSITION & DIRECTION OF WELDING

a) Position: 5G (Pipe Horizontal, Fixed Position) b) Direction of Welding: Vertical Down

Welding Procedure EPI-11-WP6 Rev. 1

Page 2 of 3

6. PREHEATING, INTERPASS TEMPERATURE & CONTROLLED COOLING

a) A minimum preheat temperature of 120°C (250°F) shall be applied to an area of at least 150 mm (6 in.) from any point to the area to be repaired. Note: The entire girth weld will be preheated to 38°C (100°F) prior to grinding repair and maintained once welding starts until repair completion.

If the interpass temperature falls below the minimum preheat temperature, the entire weld joint shall be heated to the minimum preheat temperature prior to starting the next weld pass.

The maximum interpass temperature shall not exceed 204°C (400°F).

Preheating may be applied by oxy-fuel torch, propane torch, electrical induction coils or any other method approved by Enbridge.

Preheat temperature shall be checked using temperature indicating crayons, thermocouple pyrometers or other suitable method approved by Enbridge to determine that the required preheat temperature is obtained prior to, and maintained during the welding operation.

Where applicable, precautions shall be taken through the use of insulating covers or other means to control the cooling rate of the weld after any pass.

7. POST WELD HEAT TREATMENT

Welds prepared in accordance with this specification shall not be subjected to post-weld heat treatment.

8. ELECTRICAL CHARACTERISTICS

a) Current Type: Direct Current, Reverse Polarity (DCRP) b) Amperage, Voltage and Travel Speed: See TABLE # 1 c) Heat Input: See TABLE # 1

9. TECHNIQUE

a) Minimum number of root & hot pass welders: One b) Stringer or Weave Bead:

Root & Hot Pass: String; Fill & Cap Pass: String or Weave

• Number of Weld Layers: Four weld layers minimum.

c) Cleaning methods: Hand or power tools may be used. Each pass shall be thoroughly cleaned and free of slag and scale prior to depositing the next weld layer. The completed weld shall be brushed and free of spatter.

d) Filler and Finish Beads and Finish to be Achieved: Weld repairs shall be completed in a full operation without stopping. The completed welds shall have a substantially uniform cross-section for it’s entire circumference. The crown of the weld shall not be below the surface of the adjacent base material.

10. REMOVAL AND REPAIR OF DEFECTS

Repairable defects shall be removed by grinding. The minimum length of any repair shall be 50.8 mm (2.0 in.). Welding shall be performed following the details outlines in this specification.

Welding Procedure EPI-11-WP6 Rev. 1

Page 3 of 3

11. ATTACHMENTS a) Procedure Qualification Test Records: ENB-SMAW-15.9-002-TWR

APT-SMAWRP-1 b) Laboratory Test Reports: E11-983.6

E13-491.2 c) NDT Examination Results: RTD AUT Report No. WPT-30x15.9mm-SMAW

RTD AUT Report No. APT-RMS-07 RTD RT Report No. PS12849 RTD RT Report No. PS13981 d) Material Test Report: EVRAZ Heat Number 504904

EVRAZ Heat Number 510811 TABLE # 1 WELDING PARAMETERS

Bead Number

Electrode Welding Progression

Amperage Range

amperes

Voltage Range volts

Travel Speed mm/min (in./min)

Heat Input J/mm (J/in.) Size

mm (in.) AWS Class

Root 3.2 (1/8)

or 4.0 (5/32)

E6010 Down 88 - 166 18.6 - 31 144 - 309 (5.7 - 12.2)

0.570 - 1.18 (14,478 - 29,972)

Hot 4.0 (5/32)

or 5.0 (3/16)

E8010-G Down 118 - 201 20 - 32 216 - 404 (8.5 - 15.9)

0.60 - 1.04 (15,240 - 26,416)

Fill(s) 2.4 (3/32)

or 3.2 (1/8)

E8018-C3 Up 67 - 153 17 - 28 44 - 190 (1.7 - 7.5)

0.64 - 3.54 (16,357 - 89,916)

Cap 2.4 (3/32)

or 3.2 (1/8)

E8018-C3 Up 94 - 177 17 - 28 46 - 109 (1.8 - 4.3)

1.25 - 3.26 (31,750 - 82,804)

Note – The use of stripper passes is optional.

JOINT COMPLETION AND PASS SEQUENCE:

DATE:

CODE:

914.0 mm 36.00 in.

12.8 mm 0.50 in.

WELDING POSITION:

120 °C Min 200 °C Max 120 °C Min 200 °C Max

Unknown minutes

Unknown minutes

Unknown minutes

Preheat Actual

Process in. mm °C Low High Low High mm/min IPM Low High Low High

1 Root SMAW E6010 5P+ 5/32 4.0 119 130 147 23.0 23.5 257.0 10.1 0.70 0.81 17731 20485

2 Hot SMAW E8010-G 3/16 4.8 129 160 175 26.0 26.5 257.0 10.1 0.97 1.08 24669 27500

3 Fill 1 SMAW E8018-C3 3/32 2.5 115 77 90 20.0 23.0 114.0 4.5 0.81 1.09 20454 27673

4 Fill 2 SMAW E8018-C3 1/8 3.2 115 120 123 23.0 24.0 129.0 5.1 1.28 1.37 32607 34733

5 Fill 3 SMAW E8018-C3 1/8 3.2 156 118 121 22.0 22.0 97.0 3.8 1.60 1.64 40614 41651

6 Cap 2 SMAW E8018-C3 1/8 3.2 135 113 128 21.0 21.0 91.0 3.6 1.56 1.77 39565 44841

Date:

HEAT NUMBER:

CSA Z662-11 Weld Number: APT-12.8-RP-Conf

483

Evraz

MATERIAL GRADE:

PIPE MANUFACTURER:

STRING OR WEAVE

First Fill to Completion:

Root Pass:

Hot Pass:

String

String

Weave

Root/Hot Pass:

LAB REPORT NUMBER: E13-491.2

PIPE SIZE (OD):

WALL THICKNESS:

Root Pass: 1 WELDER NAMES: 1.

510811 CSA Z662 CARBON EQUIVALENT:

ENBRIDGE PIPELINES INC.PIPELINE WELDING PROCEDURE QUALIFICATION TEST RECORD

5/1/2013 TEST LABORATORY: SGS LudwigPQR NUMBER: APT-SMAW RP-1

WELD PARAMETERS

0.27

TECHNIQUE

Hot/First Fill Pass:

JOINT DESIGN Joint Completetion and Pass SequenceJoint Geometry and Fit-Up

Fill Pass(es):

Brian Klashinsky

PREHEAT TEMP (Specified):

5G External

INTERPASS TEMP (Specified)

TYPE OF LINEUP CLAMP:

NUMBER OF WELDERS:

Heat Input

WELDING PROCESS: SMAW WELDING PROGRESSION: Downhill

Electrode Amperage Voltage

Pass

Travel Speed

Hot Pass: 1

Cap Pass(es): Weave

TIME BETWEEN PASSES:

Parameters reviewed by:

5/30/2013Name and Signature: Luke Ludwig

(J/in) (KJ/mm)Class

Diameter

30º

12.8mm

2.0mm Root Gap = 2.0 mm

MILL CERTIFICATE

Heat Pipe Test TypeCoil PM PM HAZ HAZ WMZ WMZ HAZ HAZ PMPMScale

Heat QualifiersMicrohardness Test

Customer:

Specification:

ENBRIDGE PIPELINES (ATHABASCA) INC.

CSA Z245.1-07 / ENBRIDGE SPECIFICATIONEES102-2010 REV 1

Date04/23/2013

Size: 914.400

Wall: 12.800Time

17:29:35

mm

mm

Mill OrderNo:

P4037-7297D-2WCustomer OrderNo:

70009231

MS HAZ WMZ HAZ

CertificateForm Number: L 4202

Certification Package ID: 5431

Grade: 483 CAT I

REGINA SPIRAL MILL

PM PM

L-312PrimaryChangeover:

510811 30004 QUAL INITIALB0055 237 224 226 227 231ODVickers OK

212 233 229 193 213MID

222 224 222 224 227ID

WE HEREBY CERTIFY THAT THE PRODUCTDESCRIBED ABOVE HAS PASSED ALL THE TESTSREQUIRED BY THE SPECIFICATIONS. Quality Assurance

Form: Cipr8773Measurement Taken In HV500

MS = Micro Structure

P4037-7297D-2W

Customer:

Specification:

Date: Size:

Wall:

Mill OrderNo:Customer OrderNo:

914.400 mm

12.800 mm04/23/201370009231

CSA Z245.1-07 / ENBRIDGE SPECIFICATION EES102-2010 REV 1

CertificatePackage ID:

MILL CERTIFICATECertificateForm Number:

Tensile L 4203

5431

PipeCoil OrientationTest

WidthYield

StrengthTensile

Strength Y/T(mm) (MPa)

% Elongation

(MPa) Uniform

WeldBreakTest Type

50 mm (mm)

Grade: 483 CAT I

ENBRIDGE PIPELINES (ATHABASCA) INC.

Time:17:29:41

REGINA SPIRAL MILL

L-312PrimaryChangeover:

Heat 510811

30004B0055 PIPE TPA 38.17 656512 39.0 .78QUAL INITIAL

30004B0055 PIPE TWA 38.16 727 12.0QUAL INITIAL

LRD - Longitudinal Rolling DirectionTRD - Transverse Rolling DirectionFST - Full Section (Width is the Diameter)

Form: Cipr7874

TPA - Transverse Pipe AxisLPA - Longitudinal Pipe AxisTWA - Transverse Weld Axis

WE HEREBY CERTIFY THAT THE PRODUCTDESCRIBED ABOVE HAS PASSED ALL THETESTS REQUIRED BY THE SPECIFICATIONS.

Quality Assurance

Guided Bend Tests Were Performed In Accordance WithAnd Meet The Requirements Of The Above Specification.

Hydro(%): 95.0Orientation Legend Hydrostatic Parameters

Pressure: 12900 KPAHold Time: 10 sec.

PipeCoil CType Mn S P Si Cu Ni Cr V Cb Mo Al Ca B Ti N Ce SoAlceqSn CE

P4037-7297D-2WCustomer:Specification:

Date: Size:

Wall:Mill OrderNo:

Customer OrderNo: 914.400 mm

12.800 mm04/23/2013

70009231

ENBRIDGE PIPELINES (ATHABASCA) INC.CSA Z245.1-07 / ENBRIDGE SPECIFICATION EES102-2010 REV 1

CertificatePackage ID:

MILL CERTIFICATECertificateForm Number:

Chemistry L 4201

5431

Time:17:29:30 Grade: 483 CAT I

REGINA SPIRAL MILL

L-312PrimaryChangeover:

Heat 510811

0.037HEAT 0.0000.0100.0200.00020.00340.0420.1190.0830.05 1.75 0.002 0.005 0.0010.250.070.230.31 0.007 0.27

0.03630004 PRODUCTB0055 0.0000.0100.0180.00020.00280.0420.1190.0760.05 1.73 0.002 0.008 0.0010.280.070.230.26 0.008 0.27

Form: Cipr787F

WE HEREBY CERTIFY THAT THE PRODUCTDESCRIBED ABOVE HAS PASSED ALL THETESTS REQUIRED BY THE SPECIFICATIONS.

Quality Assurance

Deoxidization Practice: Aluminum Fully KilledFurnace: ELECTRIC ARC Casting: CONTINUOUS SLAB Rolling Mill: STECKEL

ludwigl
Rectangle
ludwigl
Rectangle
ludwigl
Text Box
mis-numbered. Should be APT-12.8-RP-Conf
ludwigl
Line
ludwigl
Line
ludwigl
Line